General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 19.87 g/cm³ Show Supplier Material materials with Densidad of 19.87 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Dureza Vickers | 23.0 °C | 130 [-] Show Supplier Material materials with Dureza Vickers of 130 [-] | |
Elongación | 1200.0 °C | 28 % Show Supplier Material materials with Elongación of 28 % | |
1400.0 °C | 32 % Show Supplier Material materials with Elongación of 32 % | ||
1600.0 °C | 56 % Show Supplier Material materials with Elongación of 56 % | ||
Límite elástico Rp 0,2 | 1200.0 °C | 57 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 57 MPa | |
1400.0 °C | 40 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 40 MPa | ||
1600.0 °C | 27 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 27 MPa | ||
Módulo elástico | 1200.0 °C | 142.2 GPa Show Supplier Material materials with Módulo elástico of 142.2 GPa | |
Norton Exponent | 1200.0 °C | 6.7 [-] Show Supplier Material materials with Norton Exponent of 6.7 [-] | |
1400.0 °C | 11.6 [-] Show Supplier Material materials with Norton Exponent of 11.6 [-] | ||
1600.0 °C | 11 [-] Show Supplier Material materials with Norton Exponent of 11 [-] | ||
Resistencia a la fluencia | 1200.0 °C | 7.6 MPa Show Supplier Material materials with Resistencia a la fluencia of 7.6 MPa | 10,000 h (extrapolated data) |
1400.0 °C | 6.8 MPa Show Supplier Material materials with Resistencia a la fluencia of 6.8 MPa | 10,000 h (extrapolated data) | |
1600.0 °C | 4.6 MPa Show Supplier Material materials with Resistencia a la fluencia of 4.6 MPa | 10,000 h (extrapolated data) | |
Resistencia a la tracción | 1200.0 °C | 85 MPa Show Supplier Material materials with Resistencia a la tracción of 85 MPa | |
1400.0 °C | 52 MPa Show Supplier Material materials with Resistencia a la tracción of 52 MPa | ||
1600.0 °C | 31 MPa Show Supplier Material materials with Resistencia a la tracción of 31 MPa | ||
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Conductividad térmica | 20.0 °C | 40.3 W/(m·K) Show Supplier Material materials with Conductividad térmica of 40.3 W/(m·K) |
1200.0 °C | 66.7 W/(m·K) Show Supplier Material materials with Conductividad térmica of 66.7 W/(m·K) | |
1400.0 °C | 69.5 W/(m·K) Show Supplier Material materials with Conductividad térmica of 69.5 W/(m·K) | |
Temperatura de fusión | 1840 - 1870 °C Show Supplier Material materials with Temperatura de fusión of 1840 - 1870 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.5E-7 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.5E-7 Ω·m |
1156.0 °C | 5.5E-7 Ω·m Show Supplier Material materials with Resistividad eléctrica of 5.5E-7 Ω·m | |
1400.0 °C | 6.1E-7 Ω·m Show Supplier Material materials with Resistividad eléctrica of 6.1E-7 Ω·m | |