General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 18.74 g/cm³ Show Supplier Material materials with Densidad of 18.74 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Dureza Vickers | 23.0 °C | 99 [-] Show Supplier Material materials with Dureza Vickers of 99 [-] | |
Elongación | 20.0 °C | 43 % Show Supplier Material materials with Elongación of 43 % | |
1200.0 °C | 29 % Show Supplier Material materials with Elongación of 29 % | ||
1400.0 °C | 36 % Show Supplier Material materials with Elongación of 36 % | ||
1600.0 °C | 34 % Show Supplier Material materials with Elongación of 34 % | ||
Límite elástico Rp 0,2 | 20.0 °C | 130 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 130 MPa | |
1200.0 °C | 58.6 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 58.6 MPa | ||
1400.0 °C | 35.7 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 35.7 MPa | ||
1600.0 °C | 24.4 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 24.4 MPa | ||
Módulo elástico | 20.0 °C | 246 GPa Show Supplier Material materials with Módulo elástico of 246 GPa | |
1200.0 °C | 179 GPa Show Supplier Material materials with Módulo elástico of 179 GPa | ||
1400.0 °C | 166 GPa Show Supplier Material materials with Módulo elástico of 166 GPa | ||
1600.0 °C | 145 GPa Show Supplier Material materials with Módulo elástico of 145 GPa | ||
Norton Exponent | 1200.0 °C | 3.5 [-] Show Supplier Material materials with Norton Exponent of 3.5 [-] | |
1400.0 °C | 3.6 [-] Show Supplier Material materials with Norton Exponent of 3.6 [-] | ||
1600.0 °C | 3.5 [-] Show Supplier Material materials with Norton Exponent of 3.5 [-] | ||
Resistencia a la fluencia | 1200.0 °C | 2.8 MPa Show Supplier Material materials with Resistencia a la fluencia of 2.8 MPa | 10,000 h (extrapolated data) |
1400.0 °C | 2.2 MPa Show Supplier Material materials with Resistencia a la fluencia of 2.2 MPa | 10,000 h (extrapolated data) | |
1600.0 °C | 0.8 MPa Show Supplier Material materials with Resistencia a la fluencia of 0.8 MPa | 10,000 h (extrapolated data) | |
Resistencia a la tracción | 20.0 °C | 377 MPa Show Supplier Material materials with Resistencia a la tracción of 377 MPa | |
1200.0 °C | 92.7 MPa Show Supplier Material materials with Resistencia a la tracción of 92.7 MPa | ||
1400.0 °C | 51.4 MPa Show Supplier Material materials with Resistencia a la tracción of 51.4 MPa | ||
1600.0 °C | 27.4 MPa Show Supplier Material materials with Resistencia a la tracción of 27.4 MPa | ||
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Conductividad térmica | 20.0 °C | 34 W/(m·K) Show Supplier Material materials with Conductividad térmica of 34 W/(m·K) |
1200.0 °C | 60.7 W/(m·K) Show Supplier Material materials with Conductividad térmica of 60.7 W/(m·K) | |
1400.0 °C | 63.5 W/(m·K) Show Supplier Material materials with Conductividad térmica of 63.5 W/(m·K) | |
Temperatura de fusión | 1830 - 1855 °C Show Supplier Material materials with Temperatura de fusión of 1830 - 1855 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 2.1E-7 Ω·m Show Supplier Material materials with Resistividad eléctrica of 2.1E-7 Ω·m |
1151.0 °C | 5.2E-7 Ω·m Show Supplier Material materials with Resistividad eléctrica of 5.2E-7 Ω·m | |
1400.0 °C | 5.8E-7 Ω·m Show Supplier Material materials with Resistividad eléctrica of 5.8E-7 Ω·m | |