General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.09 % Show Material materials with Absorción de agua of 0.09 % | ISO 62 | 23°C, 50% RH |
Densidad | 23.0 °C | 1.58 g/cm³ Show Material materials with Densidad of 1.58 g/cm³ | ASTM D 792 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 2 % Show Material materials with Elongación of 2 % | ASTM D 638 | Type I, 5 mm/min |
Elongation at yield | 23.0 °C | 2 % Show Material materials with Elongation at yield of 2 % | ASTM D 638 | Type I, 5 mm/min |
Flexural strain | 23.0 °C | 3 % Show Material materials with Flexural strain of 3 % | ISO 178 | 2 mm/min |
Flexural yield strength | 23.0 °C | 160 MPa Show Material materials with Flexural yield strength of 160 MPa | ISO 178 | 2 mm/min |
Hardness, Ball Indentation | 23.0 °C | 142 MPa Show Material materials with Hardness, Ball Indentation of 142 MPa | ISO 2039-1 |
Hardness, Rockwell R | 23.0 °C | 120 [-] Show Material materials with Hardness, Rockwell R of 120 [-] | ISO 2039-2 |
Impact strength, Izod notched, ASTM | -30.0 °C | 65 J/m Show Material materials with Impact strength, Izod notched, ASTM of 65 J/m | ASTM D 256 |
23.0 °C | 70 J/m Show Material materials with Impact strength, Izod notched, ASTM of 70 J/m | ASTM D 256 | |
Impact strength, Izod unnotched, ASTM | -30.0 °C | 470 J/m Show Material materials with Impact strength, Izod unnotched, ASTM of 470 J/m | ASTM D 4812 |
23.0 °C | 530 J/m Show Material materials with Impact strength, Izod unnotched, ASTM of 530 J/m | ASTM D 4812 | |
Límite elástico | 23.0 °C | 110 MPa Show Material materials with Límite elástico of 110 MPa | ASTM D 638 | Type I, 5 mm/min |
Módulo de flexión | 23.0 °C | 7 GPa Show Material materials with Módulo de flexión of 7 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 7.8 GPa Show Material materials with Módulo elástico of 7.8 GPa | ASTM D 638 | 5 mm/min |
Resistencia a la flexión | 23.0 °C | 160 MPa Show Material materials with Resistencia a la flexión of 160 MPa | ISO 178 |
Resistencia a la tracción | 23.0 °C | 110 MPa Show Material materials with Resistencia a la tracción of 110 MPa | ASTM D 638 | Type I, 5 mm/min |
Resistencia al choque, ensayo Charpy entallado | -30.0 °C | 8 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 8 kJ/m² | ISO 179/2C |
23.0 °C | 8 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 8 kJ/m² | ISO 179/2C | |
Resistencia al choque, ensayo Charpy no entallado | -30.0 °C | 28 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy no entallado of 28 kJ/m² | ISO 179/1eU |
23.0 °C | 30 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy no entallado of 30 kJ/m² | ISO 179/1eU | |
Resistencia al choque, ensayo Izod entallado | -30.0 °C | 7 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 7 kJ/m² | ISO 180/1A |
23.0 °C | 8 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 8 kJ/m² | ISO 180/1A | |
Resistencia al choque, ensayo Izod no entallado | -30.0 °C | 30 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod no entallado of 30 kJ/m² | ISO 180/1U |
23.0 °C | 35 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod no entallado of 35 kJ/m² | ISO 180/1U | |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 2.5E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5E-5 1/K | ASTM E 831 | 23°C to 150°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 1.8E-4 1/K Show Material materials with Coeficiente de dilatación térmica transversal of 1.8E-4 1/K | ASTM E 831 | 23°C to 150°C | ||
Conductividad térmica | 23.0 °C | 0.27 W/(m·K) Show Material materials with Conductividad térmica of 0.27 W/(m·K) | ISO 8302 | ||
Heat deflection temperature, 1.80 MPa | 205 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 205 °C | ASTM D 648 | 1.82 MPa, 3.2mm, unannealed | |||
Relative temperature index, electrical | 130 °C Show Material materials with Relative temperature index, electrical of 130 °C | UL 746B | |||
Relative temperature index, mechanical impact | 130 °C Show Material materials with Relative temperature index, mechanical impact of 130 °C | UL 746B | |||
Relative temperature index, mechanical strength | 130 °C Show Material materials with Relative temperature index, mechanical strength of 130 °C | UL 746B | |||
Temperatura de reblandecimiento Vicat | 206 °C Show Material materials with Temperatura de reblandecimiento Vicat of 206 °C | ASTM D 1525 | Rate B/50 | |||
Inflamabilidad | UL Recognized, 94-5VB Flame Class Rating | 1.5mm | UL 94 |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Constante dieléctrica | 23.0 °C | 3.4 [-] Show Material materials with Constante dieléctrica of 3.4 [-] | ASTM D 150 | at 1 MHz |
Factor de disipación | 23.0 °C | 0.02 [-] Show Material materials with Factor de disipación of 0.02 [-] | ASTM D 150 | at 1 MHz |
Resistividad eléctrica | 23.0 °C | 1.00E+13 Ω·m Show Material materials with Resistividad eléctrica of 1.00E+13 Ω·m | ASTM D 257 |
Rigidez dieléctrica | 23.0 °C | 20 kV/mm Show Material materials with Rigidez dieléctrica of 20 kV/mm | ASTM D 149 | in oil, 3.2 mm |
Índice de seguimiento comparativo | 23.0 °C | 275 V Show Material materials with Índice de seguimiento comparativo of 275 V | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.3 - 0.7 % Show Material materials with Contracción of 0.3 - 0.7 % | SABIC method |
Contracción transversal | 23.0 °C | 0.6 - 0.9 % Show Material materials with Contracción transversal of 0.6 - 0.9 % | SABIC method |
Melt viscosity | 260.0 °C | 95 Pa·s Show Material materials with Melt viscosity of 95 Pa·s | ISO 11443 | 1500 sec⁻¹ |
Velocidad de flujo de la masa derretida | 26 g/10min Show Material materials with Velocidad de flujo de la masa derretida of 26 g/10min | ISO 1133 | 250°C/2.16 kg | |
Velocidad de flujo del volumen derretido | 95 cm³/10min Show Material materials with Velocidad de flujo del volumen derretido of 95 cm³/10min | ISO 1133 | 265°C/5.0 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Building Accessory,Circuit Protection,Document Handling,Electronic Components,Enclosures,Heavy Vehicles,LED Lighting,Medical Device,Meter Gas,Personal Computing,Photovoltaic Components,Wireless Communications,Wiring Devices,Wire & cable | |
Fillers | 20% Glass Fiber | |
Processing methods | Drying Temperature: 110-120°C, Drying Time: 2-4hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 250-270°C, Nozzle Temperature: 240-260°C, Front - Zone 3 Temperature: 245-265°C, Middle - Zone 2 Temperature: 240-255°C, Rear - Zone 1 Temperature: 230-245°C, Hopper Temperature: 40-60°C, Mold Temperature: 40-100°C |