General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.07 % Show Material materials with Absorción de agua of 0.07 % | ISO 62 | 23°C, 50% RH |
Densidad | 23.0 °C | 1.63 g/cm³ Show Material materials with Densidad of 1.63 g/cm³ | ASTM D 792 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 2 % Show Material materials with Elongación of 2 % | ASTM D 638 | Type I, 5 mm/min |
Elongation at yield | 23.0 °C | 2 % Show Material materials with Elongation at yield of 2 % | ASTM D 638 | Type I, 5 mm/min |
Hardness, Ball Indentation | 23.0 °C | 118 MPa Show Material materials with Hardness, Ball Indentation of 118 MPa | ISO 2039-1 |
Hardness, Rockwell R | 23.0 °C | 119 [-] Show Material materials with Hardness, Rockwell R of 119 [-] | ASTM D 785 |
Impact strength, Izod notched, ASTM | -30.0 °C | 57 J/m Show Material materials with Impact strength, Izod notched, ASTM of 57 J/m | ASTM D 256 |
23.0 °C | 60 J/m Show Material materials with Impact strength, Izod notched, ASTM of 60 J/m | ASTM D 256 | |
Impact strength, Izod unnotched, ASTM | 23.0 °C | 620 J/m Show Material materials with Impact strength, Izod unnotched, ASTM of 620 J/m | ASTM D 4812 |
Límite elástico | 23.0 °C | 120 MPa Show Material materials with Límite elástico of 120 MPa | ASTM D 638 | Type I, 5 mm/min |
Módulo de flexión | 23.0 °C | 9.5 GPa Show Material materials with Módulo de flexión of 9.5 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 12 GPa Show Material materials with Módulo elástico of 12 GPa | ASTM D 638 | 5 mm/min |
Resistencia a la flexión | 23.0 °C | 180 MPa Show Material materials with Resistencia a la flexión of 180 MPa | ISO 178 |
Resistencia a la tracción | 23.0 °C | 120 MPa Show Material materials with Resistencia a la tracción of 120 MPa | ASTM D 638 | Type I, 5 mm/min |
Resistencia al choque, ensayo Charpy entallado | -30.0 °C | 6 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 6 kJ/m² | ISO 179/1eA |
23.0 °C | 7 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 7 kJ/m² | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -30.0 °C | 50 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy no entallado of 50 kJ/m² | ISO 179/1eU |
23.0 °C | 50 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy no entallado of 50 kJ/m² | ISO 179/1eU | |
Resistencia al choque, ensayo Izod entallado | -30.0 °C | 6 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 6 kJ/m² | ISO 180/1A |
23.0 °C | 7 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 7 kJ/m² | ISO 180/1A | |
Resistencia al choque, ensayo Izod no entallado | -30.0 °C | 45 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod no entallado of 45 kJ/m² | ISO 180/1U |
23.0 °C | 45 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod no entallado of 45 kJ/m² | ISO 180/1U | |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 2.5E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2.5E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 8.9E-5 1/K Show Material materials with Coeficiente de dilatación térmica transversal of 8.9E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Conductividad térmica | 23.0 °C | 0.25 W/(m·K) Show Material materials with Conductividad térmica of 0.25 W/(m·K) | ISO 8302 | ||
Heat deflection temperature, 1.80 MPa | 200 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 200 °C | ASTM D 648 | 1.82 MPa, 3.2mm, unannealed | |||
Relative temperature index, electrical | 130 °C Show Material materials with Relative temperature index, electrical of 130 °C | UL 746B | |||
Relative temperature index, mechanical impact | 130 °C Show Material materials with Relative temperature index, mechanical impact of 130 °C | UL 746B | |||
Relative temperature index, mechanical strength | 140 °C Show Material materials with Relative temperature index, mechanical strength of 140 °C | UL 746B | |||
Temperatura de reblandecimiento Vicat | 200 °C Show Material materials with Temperatura de reblandecimiento Vicat of 200 °C | ASTM D 1525 | Rate B/50 | |||
Inflamabilidad | UL Recognized, 94-5VA Flame Class Rating | 2mm | UL 94 |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Constante dieléctrica | 23.0 °C | 3.7 [-] Show Material materials with Constante dieléctrica of 3.7 [-] | ASTM D 150 | at 1 MHz |
Factor de disipación | 23.0 °C | 0.02 [-] Show Material materials with Factor de disipación of 0.02 [-] | ASTM D 150 | at 1 MHz |
Rigidez dieléctrica | 23.0 °C | 24 kV/mm Show Material materials with Rigidez dieléctrica of 24 kV/mm | ASTM D 149 | in oil, 1.6 mm |
Índice de seguimiento comparativo | 23.0 °C | 175 V Show Material materials with Índice de seguimiento comparativo of 175 V | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.5 - 0.7 % Show Material materials with Contracción of 0.5 - 0.7 % | SABIC method | 3.2 mm |
Contracción transversal | 23.0 °C | 0.5 - 1 % Show Material materials with Contracción transversal of 0.5 - 1 % | SABIC method |
Velocidad de flujo de la masa derretida | 42 g/10min Show Material materials with Velocidad de flujo de la masa derretida of 42 g/10min | ASTM D 1238 | 250°C/5.0 kgf | |
Velocidad de flujo del volumen derretido | 29 cm³/10min Show Material materials with Velocidad de flujo del volumen derretido of 29 cm³/10min | ISO 1133 | 250°C/5.0 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Air Cabin Interiors,Air Conditioning,ATM/Ticket Machine,Audio,Auto Aftermarket,Building Accessory,Circuit Protection,Cladding,Cladding/Roof,Coffee Maker/Espresso Machine,Commercial Storage/Cookware,Cooking Range,Data Management,Data Transfer,Dishwasher,Displays,Document Handling,Doors Hardware/Trim,Electronic Components,Enclosure/Housing/Cover,Enclosures,Energy Management,EV Infrastructure,Exterior Mirror,Food Processor,Forward Lighting,Gas/Electric Oven,Heavy Vehicles,HVAC Underhood,Industrial Material Handling,Lab Ware and Clinical Diagnostics,Laundry Dryer,LED Lighting,Medical Device,Medical Facility Infrastructure,Meter Gas,Meter Water,Monitoring and Imaging,Motorcycle,Non-LED Lighting,Personal Care,Personal Computing,Photovoltaic Components,Pipe/Fitting,Plumbing,Power Boat,Power Manangement,Pump,Recreational Vehicle,Refrigerator,Security/Detection,Small Appliance,Toy,Vacuum Cleaner,Water Treatment/Filtration,Wearables,Wireless Communications,Wiring Devices,Wire & cable | |
Fillers | 30% Glass Fiber | |
Processing methods | Drying Temperature: 120°C, Drying Time: 3-4hrs, Drying Time (Cumulative): 12hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 255-275°C, Nozzle Temperature: 250-270°C, Front - Zone 3 Temperature: 255-275°C, Middle - Zone 2 Temperature: 250-270°C, Rear - Zone 1 Temperature: 245-265°C, Mold Temperature: 65-90°C, Back Pressure: 0.3-0.7MPa, Screw Speed: 50-80rpm, Shot to Cylinder Size: 40-80%, Vent Depth: 0.025-0.038mm |