General
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 35 % Show Material materials with Elongación of 35 % | ASTM D 638 | Type I, 50 mm/min |
Elongation at yield | 23.0 °C | 4.9 % Show Material materials with Elongation at yield of 4.9 % | ASTM D 638 | Type I, 50 mm/min |
Flexural yield strength | 23.0 °C | 100 MPa Show Material materials with Flexural yield strength of 100 MPa | ISO 178 | 2 mm/min |
Hardness, Ball Indentation | 23.0 °C | 113 MPa Show Material materials with Hardness, Ball Indentation of 113 MPa | ISO 2039-1 |
Hardness, Rockwell R | 23.0 °C | 124 [-] Show Material materials with Hardness, Rockwell R of 124 [-] | ISO 2039-2 |
Impact strength, Izod notched, ASTM | 23.0 °C | 694 J/m Show Material materials with Impact strength, Izod notched, ASTM of 694 J/m | ASTM D 256 |
Límite elástico | 23.0 °C | 64 MPa Show Material materials with Límite elástico of 64 MPa | ASTM D 638 | Type I, 50 mm/min |
Módulo de flexión | 23.0 °C | 2.7 GPa Show Material materials with Módulo de flexión of 2.7 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 2.86 GPa Show Material materials with Módulo elástico of 2.86 GPa | ASTM D 638 | 50 mm/min |
Resistencia a la tracción | 23.0 °C | 51 MPa Show Material materials with Resistencia a la tracción of 51 MPa | ASTM D 638 | Type I, 50 mm/min |
Resistencia al choque, ensayo Charpy entallado | -30.0 °C | 13 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 13 kJ/m² | ISO 179/1eA |
23.0 °C | 48 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 48 kJ/m² | ISO 179/1eA | |
Resistencia al choque, ensayo Izod entallado | -30.0 °C | 13 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 13 kJ/m² | ISO 180/1A |
23.0 °C | 15 - 45 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 15 - 45 kJ/m² | ISO 180/1A | |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 7.2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 7.2E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 7.2E-5 1/K Show Material materials with Coeficiente de dilatación térmica transversal of 7.2E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Conductividad térmica | 23.0 °C | 0.2 W/(m·K) Show Material materials with Conductividad térmica of 0.2 W/(m·K) | ISO 8302 | ||
Heat deflection temperature, 1.80 MPa | 88 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 88 °C | ASTM D 648 | 1.82 MPa, 3.2mm, unannealed | |||
Relative temperature index, electrical | 60 °C Show Material materials with Relative temperature index, electrical of 60 °C | UL 746B | |||
Relative temperature index, mechanical impact | 60 °C Show Material materials with Relative temperature index, mechanical impact of 60 °C | UL 746B | |||
Relative temperature index, mechanical strength | 60 °C Show Material materials with Relative temperature index, mechanical strength of 60 °C | UL 746B | |||
Temperatura de fusión | 225 - 250 °C Show Material materials with Temperatura de fusión of 225 - 250 °C | ||||
Temperatura de reblandecimiento Vicat | 110 °C Show Material materials with Temperatura de reblandecimiento Vicat of 110 °C | ASTM D 1525 | Rate B/50 | |||
Inflamabilidad | UL Recognized, 94-5VB Flame Class Rating | 2.5mm | UL 94 |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Constante dieléctrica | 23.0 °C | 2.8 [-] Show Material materials with Constante dieléctrica of 2.8 [-] | IEC 60250 | at 50/60 Hz |
Factor de disipación | 23.0 °C | 6E-3 [-] Show Material materials with Factor de disipación of 6E-3 [-] | ASTM D 150 | at 50/60 Hz |
Rigidez dieléctrica | 23.0 °C | 17 kV/mm Show Material materials with Rigidez dieléctrica of 17 kV/mm | IEC 60243-1 | in oil, 3.2 mm |
Índice de seguimiento comparativo | 23.0 °C | 600 V Show Material materials with Índice de seguimiento comparativo of 600 V | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.4 - 0.6 % Show Material materials with Contracción of 0.4 - 0.6 % | SABIC method | 3.2 mm |
Velocidad de flujo de la masa derretida | 8.5 g/10min Show Material materials with Velocidad de flujo de la masa derretida of 8.5 g/10min | ASTM D 1238 | 260°C/5.0 kgf | |
Velocidad de flujo del volumen derretido | 8 cm³/10min Show Material materials with Velocidad de flujo del volumen derretido of 8 cm³/10min | ISO 1133 | 260°C/5.0 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Building Element,Circuit Protection,Document Handling,Electronic Components,Enclosures,Energy Management,Headliner,Heavy Vehicles,Medical Device,Meter Gas,Power Manangement,Rail,Refrigerator,Wireless Communications,Wiring Devices,Wire & cable | |
Processing methods | Drying Temperature: 80-90°C, Drying Time: 3-4hrs, Drying Time (Cumulative): 8hrs, Maximum Moisture Content: 0.04%, Melt Temperature: 245-275°C, Nozzle Temperature: 245-275°C, Front - Zone 3 Temperature: 245-275°C, Middle - Zone 2 Temperature: 220-265°C, Rear - Zone 1 Temperature: 220-255°C, Mold Temperature: 60-80°C, Back Pressure: 0.3-0.7MPa, Screw Speed: 40-70rpm, Shot to Cylinder Size: 30-80%, Vent Depth: 0.038-0.076mm, Drying Temperature: 80-90°C, Drying Time: 2-4hrs, Drying Time (Cumulative): 8hrs, Maximum Moisture Content: 0-0.02%, Barrel - Zone 1 Temperature: 205-230°C, Barrel - Zone 2 Temperature: 215-245°C, Barrel - Zone 3 Temperature: 215-245°C, Barrel - Zone 4 Temperature: 220-250°C, Adapter - Zone 5 Temperature: 225-250°C, Head - Zone 6 - Top Temperature: 225-250°C, Head - Zone 7 - Bottom Temperature: 225-250°C, Mold Temperature: 65-90°C, Die Temperature: 240-250°C, Drying Temperature: 80-90°C, Drying Time: 2-4hrs, Drying Time (Cumulative): 8hrs, Minimum Moisture Content: 0-0.02%, Melt Temperature: 225-270°C, Barrel - Zone 1 Temperature: 205-250°C, Barrel - Zone 2 Temperature: 215-260°C, Barrel - Zone 3 Temperature: 215-260°C, Barrel - Zone 4 Temperature: 225-270°C, Adapter Temperature: 225-270°C, Die Temperature: 225-270°C |