General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.05 % Show Material materials with Absorción de agua of 0.05 % | ISO 62 | 23°C, 50% RH |
Densidad | 23.0 °C | 1.25 g/cm³ Show Material materials with Densidad of 1.25 g/cm³ | ASTM D 792 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 55 % Show Material materials with Elongación of 55 % | ASTM D 638 | Type I, 5 mm/min |
Elongation at yield | 23.0 °C | 3.4 % Show Material materials with Elongation at yield of 3.4 % | ASTM D 638 | Type I, 5 mm/min |
Flexural yield strength | 23.0 °C | 90 MPa Show Material materials with Flexural yield strength of 90 MPa | ISO 178 | 2 mm/min |
Impact strength, Izod notched, ASTM | -30.0 °C | 90 J/m Show Material materials with Impact strength, Izod notched, ASTM of 90 J/m | ASTM D 256 |
23.0 °C | 250 J/m Show Material materials with Impact strength, Izod notched, ASTM of 250 J/m | ASTM D 256 | |
Impact strength, Izod unnotched, ASTM | -30.0 °C | 1450 J/m Show Material materials with Impact strength, Izod unnotched, ASTM of 1450 J/m | ASTM D 4812 |
23.0 °C | 1650 J/m Show Material materials with Impact strength, Izod unnotched, ASTM of 1650 J/m | ASTM D 4812 | |
Límite elástico | 23.0 °C | 47 MPa Show Material materials with Límite elástico of 47 MPa | ASTM D 638 | Type I, 5 mm/min |
Módulo de flexión | 23.0 °C | 3.6 GPa Show Material materials with Módulo de flexión of 3.6 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 3.6 GPa Show Material materials with Módulo elástico of 3.6 GPa | ASTM D 638 | 5 mm/min |
Resistencia a la tracción | 23.0 °C | 60 MPa Show Material materials with Resistencia a la tracción of 60 MPa | ASTM D 638 | Type I, 5 mm/min |
Resistencia al choque, ensayo Charpy entallado | -30.0 °C | 8 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 8 kJ/m² | ISO 179/2C |
23.0 °C | 12 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 12 kJ/m² | ISO 179/2C | |
Resistencia al choque, ensayo Charpy no entallado | -30.0 °C | 100 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy no entallado of 100 kJ/m² | ISO 179/1eU |
23.0 °C | 105 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy no entallado of 105 kJ/m² | ISO 179/1eU | |
Resistencia al choque, ensayo Izod entallado | -30.0 °C | 8 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 8 kJ/m² | ISO 180/1A |
23.0 °C | 13 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 13 kJ/m² | ISO 180/1A | |
Resistencia al choque, ensayo Izod no entallado | -30.0 °C | 135 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod no entallado of 135 kJ/m² | ISO 180/1U |
23.0 °C | 140 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod no entallado of 140 kJ/m² | ISO 180/1U | |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 5.6E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 5.6E-5 1/K | ISO 11359-2 | -30°C to 80°C |
Coeficiente de dilatación térmica transversal | 23.0 °C | 7E-5 1/K Show Material materials with Coeficiente de dilatación térmica transversal of 7E-5 1/K | ISO 11359-2 | -30°C to 80°C |
Heat deflection temperature, 0.45 MPa | 129 °C Show Material materials with Heat deflection temperature, 0.45 MPa of 129 °C | ISO 75/Bf | 0.45 MPa | |
Temperatura de reblandecimiento Vicat | 134 °C Show Material materials with Temperatura de reblandecimiento Vicat of 134 °C | ISO 306 | Rate B/120 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.4 - 0.6 % Show Material materials with Contracción of 0.4 - 0.6 % | SABIC method | 3.2 mm |
Contracción transversal | 23.0 °C | 0.3 - 0.5 % Show Material materials with Contracción transversal of 0.3 - 0.5 % | SABIC method |
Velocidad de flujo de la masa derretida | 16 g/10min Show Material materials with Velocidad de flujo de la masa derretida of 16 g/10min | ASTM D 1238 | 260°C/5.0 kgf | |
Velocidad de flujo del volumen derretido | 15 cm³/10min Show Material materials with Velocidad de flujo del volumen derretido of 15 cm³/10min | ISO 1133 | 260°C/5.0 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Console,Exterior Trim,Spoiler,Trim | |
Processing methods | Drying Temperature: 110-120°C, Drying Time: 2-6hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 270-300°C, Nozzle Temperature: 260-290°C, Front - Zone 3 Temperature: 270-300°C, Middle - Zone 2 Temperature: 265-290°C, Rear - Zone 1 Temperature: 260-270°C, Mold Temperature: 60-100°C, Back Pressure: 0.3-0.7MPa, Screw Speed: 40-70rpm, Shot to Cylinder Size: 30-80%, Vent Depth: 0.038-0.076mm |