General
Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 1.2 g/cm³ Show Material materials with Densidad of 1.2 g/cm³ | ASTM D 792 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 9 % Show Material materials with Elongación of 9 % | ASTM D 638 | Type I, 5 mm/min |
Elongation at yield | 23.0 °C | 2.3 % Show Material materials with Elongation at yield of 2.3 % | ASTM D 638 | Type I, 5 mm/min |
Flexural yield strength | 23.0 °C | 71 MPa Show Material materials with Flexural yield strength of 71 MPa | ASTM D 790 | 1.3 mm/min, 50 mm span |
Impact strength, Izod notched, ASTM | 23.0 °C | 213 J/m Show Material materials with Impact strength, Izod notched, ASTM of 213 J/m | ASTM D 256 |
Límite elástico | 23.0 °C | 41 MPa Show Material materials with Límite elástico of 41 MPa | ASTM D 638 | Type I, 5 mm/min |
Módulo de flexión | 23.0 °C | 2.72 GPa Show Material materials with Módulo de flexión of 2.72 GPa | ASTM D 790 | 1.3 mm/min, 50 mm span |
Módulo elástico | 23.0 °C | 2.34 GPa Show Material materials with Módulo elástico of 2.34 GPa | ASTM D 638 | 5 mm/min |
Resistencia a la tracción | 23.0 °C | 35 MPa Show Material materials with Resistencia a la tracción of 35 MPa | ASTM D 638 | Type I, 5 mm/min |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 8.46E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 8.46E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 8.64E-5 1/K Show Material materials with Coeficiente de dilatación térmica transversal of 8.64E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Heat deflection temperature, 1.80 MPa | 70 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 70 °C | ASTM D 648 | 1.82 MPa, 3.2mm, unannealed | |||
Relative temperature index, electrical | 60 °C Show Material materials with Relative temperature index, electrical of 60 °C | UL 746B | |||
Relative temperature index, mechanical impact | 60 °C Show Material materials with Relative temperature index, mechanical impact of 60 °C | UL 746B | |||
Relative temperature index, mechanical strength | 60 °C Show Material materials with Relative temperature index, mechanical strength of 60 °C | UL 746B | |||
Temperatura de reblandecimiento Vicat | 86 °C Show Material materials with Temperatura de reblandecimiento Vicat of 86 °C | ASTM D 1525 | Rate B/50 | |||
Inflamabilidad | UL Recognized, 94-5VA Flame Class Rating | 2.48mm | UL 94 |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Índice de seguimiento comparativo | 23.0 °C | 2 V Show Material materials with Índice de seguimiento comparativo of 2 V | UL 746A |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.5 - 0.7 % Show Material materials with Contracción of 0.5 - 0.7 % | SABIC method | 3.2 mm |
Melt viscosity | 23.0 °C | 290 Pa·s Show Material materials with Melt viscosity of 290 Pa·s | ASTM D 3825 | 200°C, 1000 sec⁻¹ |
Velocidad de flujo de la masa derretida | 10 g/10min Show Material materials with Velocidad de flujo de la masa derretida of 10 g/10min | ISO 1133 | 220°C/5.0 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Air Conditioning,Audio,Building Accessory,Circuit Protection,Data Management,Data Transfer,Defense Vehicles,Dishwasher,Document Handling,Electronic Components,Enclosure/Housing/Cover,Enclosures,Energy Management,Fixture Bath/Shower,Furnace/Heater,Gas/Electric Oven,Lab Ware and Clinical Diagnostics,Laundry Dryer,Medical Device,Medical Facility Infrastructure,Microwave Oven,Modular Panel,Monitoring and Imaging,Non-LED Lighting,Personal Computing,Photo/Video Camera,Power Manangement,Refrigerator,Respiratory,Security/Detection,Small Appliance,Surgical Devices,Washing Machine,Water Treatment/Filtration,Wireless Communications,Wiring Devices | |
Processing methods | Drying Temperature: 80-90°C, Drying Time: 2-4hrs, Drying Time (Cumulative): 6hrs, Maximum Moisture Content: 0.1%, Melt Temperature: 200-220°C, Nozzle Temperature: 200-220°C, Front - Zone 3 Temperature: 200-215°C, Middle - Zone 2 Temperature: 195-205°C, Rear - Zone 1 Temperature: 170-180°C, Mold Temperature: 50-70°C, Back Pressure: 0.3-0.7MPa, Screw Speed: 30-60rpm, Shot to Cylinder Size: 50-70%, Vent Depth: 0.038-0.051mm |