General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.2 % Show Material materials with Absorción de agua of 0.2 % | ISO 62 | 23°C, 50% RH |
Densidad | 23.0 °C | 1.17 g/cm³ Show Material materials with Densidad of 1.17 g/cm³ | ISO 1183 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongation at yield | 23.0 °C | 4.2 % Show Material materials with Elongation at yield of 4.2 % | ASTM D 638 | Type I, 5 mm/min |
Flexural yield strength | 23.0 °C | 93 MPa Show Material materials with Flexural yield strength of 93 MPa | ISO 178 | 2 mm/min |
Impact strength, Izod notched, ASTM | 23.0 °C | 385 J/m Show Material materials with Impact strength, Izod notched, ASTM of 385 J/m | ASTM D 256 |
Límite elástico | 23.0 °C | 59 MPa Show Material materials with Límite elástico of 59 MPa | ASTM D 638 | Type I, 5 mm/min |
Módulo de flexión | 23.0 °C | 2.51 GPa Show Material materials with Módulo de flexión of 2.51 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 2.59 GPa Show Material materials with Módulo elástico of 2.59 GPa | ASTM D 638 | 5 mm/min |
Resistencia a la tracción | 23.0 °C | 66 MPa Show Material materials with Resistencia a la tracción of 66 MPa | ASTM D 638 | Type I, 5 mm/min |
Resistencia al choque, ensayo Charpy entallado | 23.0 °C | 15 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 15 kJ/m² | ISO 179/1eA |
Resistencia al choque, ensayo Izod entallado | -30.0 °C | 9 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 9 kJ/m² | ISO 180/1A |
23.0 °C | 12 - 17 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 12 - 17 kJ/m² | ISO 180/1A | |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 6.9E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 6.9E-5 1/K | ISO 11359-2 | -30°C to 80°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 7.5E-5 1/K Show Material materials with Coeficiente de dilatación térmica transversal of 7.5E-5 1/K | ISO 11359-2 | 23°C to 80°C | ||
Heat deflection temperature, 1.80 MPa | 88 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 88 °C | ISO 75/Ae | 1.8 MPa | |||
Temperatura de reblandecimiento Vicat | 104 °C Show Material materials with Temperatura de reblandecimiento Vicat of 104 °C | ISO 306 | Rate B/120 | |||
Inflamabilidad | UL Compliant, 94V-0 Flame Class Rating | 2mm | UL 94 by SABIC-IP |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.4 - 0.6 % Show Material materials with Contracción of 0.4 - 0.6 % | SABIC method |
Velocidad de flujo del volumen derretido | 13 cm³/10min Show Material materials with Velocidad de flujo del volumen derretido of 13 cm³/10min | ISO 1133 | 260°C/2.16 kg |
Technological properties
Property | ||
---|---|---|
Application areas | ATM/Ticket Machine,Audio,Building Element,Building/Construction Sheet,Circuit Protection,Data Transfer,Displays,Document Handling,Electronic Components,Enclosure/Housing/Cover,Enclosures,Energy Management,LED Lighting,Medical Device,Meter Water,Personal Computing,Photo/Video Camera,Pump,Refrigerator,Security/Detection,Small Appliance,Surgical Devices,Swimming Pool/Spa,Vacuum Cleaner,Wireless Communications,Wiring Devices,Wire & cable | |
Processing methods | Drying Temperature: 80-90°C, Drying Time: 2-4hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 230-270°C, Nozzle Temperature: 220-260°C, Front - Zone 3 Temperature: 230-270°C, Middle - Zone 2 Temperature: 220-260°C, Rear - Zone 1 Temperature: 200-230°C, Hopper Temperature: 60-80°C, Mold Temperature: 50-70°C |