General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.05 % Show Material materials with Absorción de agua of 0.05 % | ISO 62 | 23°C, 50% RH |
Densidad | 23.0 °C | 1.21 g/cm³ Show Material materials with Densidad of 1.21 g/cm³ | ASTM D 792 |
Mecánica
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Elongación | 23.0 °C | 150 % Show Material materials with Elongación of 150 % | ASTM D 638 | Type I, 50 mm/min | ||
Elongation at yield | 23.0 °C | 4 % Show Material materials with Elongation at yield of 4 % | ASTM D 638 | Type I, 50 mm/min | ||
Flexural yield strength | 23.0 °C | 64 MPa Show Material materials with Flexural yield strength of 64 MPa | ISO 178 | 2 mm/min | ||
Impact strength, Izod notched, ASTM | -30.0 °C | 750 J/m Show Material materials with Impact strength, Izod notched, ASTM of 750 J/m | ASTM D 256 | ||
23.0 °C | 800 J/m Show Material materials with Impact strength, Izod notched, ASTM of 800 J/m | ASTM D 256 | |||
Límite elástico | 23.0 °C | 43 MPa Show Material materials with Límite elástico of 43 MPa | ASTM D 638 | Type I, 50 mm/min | ||
Módulo de flexión | 23.0 °C | 1.8 GPa Show Material materials with Módulo de flexión of 1.8 GPa | ISO 178 | 2 mm/min | ||
Módulo elástico | 23.0 °C | 1.9 GPa Show Material materials with Módulo elástico of 1.9 GPa | ASTM D 638 | 5 mm/min | ||
Resistencia a la tracción | 23.0 °C | 35 MPa Show Material materials with Resistencia a la tracción of 35 MPa | ASTM D 638 | Type I, 50 mm/min | ||
Resistencia al choque, ensayo Charpy entallado | 23.0 °C | 70 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 70 kJ/m² | ISO 179/1eA | ||
Resistencia al choque, ensayo Izod entallado | -30.0 °C | 20 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 20 kJ/m² | ISO 180/1A | ||
23.0 °C | 65 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 65 kJ/m² | ISO 180/1A | |||
Resistencia al choque, ensayo Charpy no entallado | No break @ -30°C | ISO 179/2C | ||||
Resistencia al choque, ensayo Izod no entallado | No break @ -40°C | ISO 180/1U |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 1E-4 1/K Show Material materials with Coeficiente de dilatación térmica of 1E-4 1/K | ASTM E 831 | -40°C to 40°C |
Coeficiente de dilatación térmica transversal | 23.0 °C | 1E-4 1/K Show Material materials with Coeficiente de dilatación térmica transversal of 1E-4 1/K | ASTM E 831 | -40°C to 40°C |
Heat deflection temperature, 0.45 MPa | 95 °C Show Material materials with Heat deflection temperature, 0.45 MPa of 95 °C | ISO 75/Bf | 0.45 MPa | |
Temperatura de reblandecimiento Vicat | 117 °C Show Material materials with Temperatura de reblandecimiento Vicat of 117 °C | ASTM D 1525 | Rate B/50 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 1.2 - 1.6 % Show Material materials with Contracción of 1.2 - 1.6 % | SABIC method | 3.2 mm |
Melt viscosity | 260.0 °C | 210 Pa·s Show Material materials with Melt viscosity of 210 Pa·s | ISO 11443 | 1500 sec⁻¹ |
Velocidad de flujo de la masa derretida | 11 g/10min Show Material materials with Velocidad de flujo de la masa derretida of 11 g/10min | ASTM D 1238 | 250°C/5.0 kgf | |
Velocidad de flujo del volumen derretido | 10 cm³/10min Show Material materials with Velocidad de flujo del volumen derretido of 10 cm³/10min | ISO 1133 | 250°C/5.0 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Medical Device,Monitoring and Imaging | |
Processing methods | Drying Temperature: 90-100°C, Drying Time: 2-4hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 255-270°C, Nozzle Temperature: 250-265°C, Front - Zone 3 Temperature: 250-270°C, Middle - Zone 2 Temperature: 240-265°C, Rear - Zone 1 Temperature: 230-250°C, Hopper Temperature: 40-60°C, Mold Temperature: 60-80°C |