General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.15 % Show Material materials with Absorción de agua of 0.15 % | ISO 62 | 23°C, 50% RH |
Densidad | 23.0 °C | 1.19 g/cm³ Show Material materials with Densidad of 1.19 g/cm³ | ASTM D 792 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 125 % Show Material materials with Elongación of 125 % | ASTM D 638 | Type I, 50 mm/min |
Elongation at yield | 23.0 °C | 6 % Show Material materials with Elongation at yield of 6 % | ASTM D 638 | Type I, 50 mm/min |
Flexural yield strength | 23.0 °C | 90 MPa Show Material materials with Flexural yield strength of 90 MPa | ISO 178 | 2 mm/min |
Impact strength, Izod notched, ASTM | 23.0 °C | 801 J/m Show Material materials with Impact strength, Izod notched, ASTM of 801 J/m | ASTM D 256 |
Límite elástico | 23.0 °C | 62 MPa Show Material materials with Límite elástico of 62 MPa | ASTM D 638 | Type I, 50 mm/min |
Módulo de flexión | 23.0 °C | 2.3 GPa Show Material materials with Módulo de flexión of 2.3 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 2.27 GPa Show Material materials with Módulo elástico of 2.27 GPa | ASTM D 638 | 50 mm/min |
Resistencia a la tracción | 23.0 °C | 67 MPa Show Material materials with Resistencia a la tracción of 67 MPa | ASTM D 638 | Type I, 50 mm/min |
Resistencia al choque, ensayo Izod entallado | 23.0 °C | 10 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 10 kJ/m² | ISO 180/1A |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 6.84E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 6.84E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 7.38E-5 1/K Show Material materials with Coeficiente de dilatación térmica transversal of 7.38E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Heat deflection temperature, 1.80 MPa | 126 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 126 °C | ASTM D 648 | 1.82 MPa, 3.2mm, unannealed | |||
Relative temperature index, electrical | 130 °C Show Material materials with Relative temperature index, electrical of 130 °C | UL 746B | |||
Relative temperature index, mechanical impact | 120 °C Show Material materials with Relative temperature index, mechanical impact of 120 °C | UL 746B | |||
Relative temperature index, mechanical strength | 130 °C Show Material materials with Relative temperature index, mechanical strength of 130 °C | UL 746B | |||
Temperatura de reblandecimiento Vicat | 143 °C Show Material materials with Temperatura de reblandecimiento Vicat of 143 °C | ASTM D 1525 | Rate B/50 | |||
Inflamabilidad | UL Recognized, 94V-0 Flame Class Rating | 3.05mm | UL 94 |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Constante dieléctrica | 23.0 °C | 2.7 [-] Show Material materials with Constante dieléctrica of 2.7 [-] | ASTM D 150 | at 1 MHz |
Factor de disipación | 23.0 °C | 0.01 [-] Show Material materials with Factor de disipación of 0.01 [-] | ASTM D 150 | at 1 MHz |
Rigidez dieléctrica | 23.0 °C | 17 kV/mm Show Material materials with Rigidez dieléctrica of 17 kV/mm | ASTM D 149 | in oil, 3.2 mm |
Índice de seguimiento comparativo | 23.0 °C | 3 V Show Material materials with Índice de seguimiento comparativo of 3 V | UL 746A |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.6 - 0.8 % Show Material materials with Contracción of 0.6 - 0.8 % | SABIC method | 3.2 mm |
Velocidad de flujo de la masa derretida | 14 g/10min Show Material materials with Velocidad de flujo de la masa derretida of 14 g/10min | ASTM D 1238 | 300°C/1.2 kg | |
Velocidad de flujo del volumen derretido | 13 cm³/10min Show Material materials with Velocidad de flujo del volumen derretido of 13 cm³/10min | ISO 1133 | 300°C/1.2 kg |
Technological properties
Property | ||
---|---|---|
Application areas | EV Infrastructure,LED Lighting,Non-LED Lighting | |
Processing methods | Drying Temperature: 120°C, Drying Time: 2-4hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 280-310°C, Nozzle Temperature: 270-290°C, Front - Zone 3 Temperature: 280-310°C, Middle - Zone 2 Temperature: 270-290°C, Rear - Zone 1 Temperature: 260-280°C, Hopper Temperature: 60-80°C, Mold Temperature: 80-110°C |