General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.23 % Show Material materials with Absorción de agua of 0.23 % | ISO 62 | 23°C, 50% RH |
Densidad | 23.0 °C | 1.46 g/cm³ Show Material materials with Densidad of 1.46 g/cm³ | ASTM D 792 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 2.8 % Show Material materials with Elongación of 2.8 % | ASTM D 638 | Type I, 5 mm/min |
Elongation at yield | 23.0 °C | 2.8 % Show Material materials with Elongation at yield of 2.8 % | ASTM D 638 | Type I, 5 mm/min |
Flexural strain | 23.0 °C | 2.9 % Show Material materials with Flexural strain of 2.9 % | ISO 178 | 2 mm/min |
Flexural yield strength | 23.0 °C | 185 MPa Show Material materials with Flexural yield strength of 185 MPa | ISO 178 | 2 mm/min |
Hardness, Ball Indentation | 23.0 °C | 210 MPa Show Material materials with Hardness, Ball Indentation of 210 MPa | ISO 2039-1 |
Hardness, Rockwell R | 23.0 °C | 116 [-] Show Material materials with Hardness, Rockwell R of 116 [-] | ISO 2039-2 |
Impact strength, Izod notched, ASTM | -30.0 °C | 80 J/m Show Material materials with Impact strength, Izod notched, ASTM of 80 J/m | ASTM D 256 |
23.0 °C | 80 J/m Show Material materials with Impact strength, Izod notched, ASTM of 80 J/m | ASTM D 256 | |
Impact strength, Izod unnotched, ASTM | -30.0 °C | 800 J/m Show Material materials with Impact strength, Izod unnotched, ASTM of 800 J/m | ASTM D 4812 |
23.0 °C | 800 J/m Show Material materials with Impact strength, Izod unnotched, ASTM of 800 J/m | ASTM D 4812 | |
Límite elástico | 23.0 °C | 125 MPa Show Material materials with Límite elástico of 125 MPa | ASTM D 638 | Type I, 5 mm/min |
Módulo de flexión | 23.0 °C | 8.2 GPa Show Material materials with Módulo de flexión of 8.2 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 9.5 GPa Show Material materials with Módulo elástico of 9.5 GPa | ASTM D 638 | 5 mm/min |
Resistencia a la flexión | 23.0 °C | 180 MPa Show Material materials with Resistencia a la flexión of 180 MPa | ISO 178 |
Resistencia a la tracción | 23.0 °C | 125 MPa Show Material materials with Resistencia a la tracción of 125 MPa | ASTM D 638 | Type I, 5 mm/min |
Resistencia al choque, ensayo Charpy entallado | -30.0 °C | 9 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 9 kJ/m² | ISO 179/2C |
23.0 °C | 9 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 9 kJ/m² | ISO 179/2C | |
Resistencia al choque, ensayo Charpy no entallado | -30.0 °C | 25 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy no entallado of 25 kJ/m² | ISO 179/1eU |
23.0 °C | 30 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy no entallado of 30 kJ/m² | ISO 179/1eU | |
Resistencia al choque, ensayo Izod entallado | -30.0 °C | 8 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 8 kJ/m² | ISO 180/1A |
23.0 °C | 8 - 9 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 8 - 9 kJ/m² | ISO 180/1A | |
Resistencia al choque, ensayo Izod no entallado | -30.0 °C | 45 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod no entallado of 45 kJ/m² | ISO 180/1U |
23.0 °C | 50 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod no entallado of 50 kJ/m² | ISO 180/1U | |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 2.2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2E-5 1/K | ASTM E 831 | -40°C to 40°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 1.15E-4 1/K Show Material materials with Coeficiente de dilatación térmica transversal of 1.15E-4 1/K | ASTM E 831 | -40°C to 40°C | ||
Conductividad térmica | 23.0 °C | 0.26 W/(m·K) Show Material materials with Conductividad térmica of 0.26 W/(m·K) | ISO 8302 | ||
Heat deflection temperature, 1.80 MPa | 190 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 190 °C | ASTM D 648 | 1.82 MPa, 3.2mm, unannealed | |||
Relative temperature index, electrical | 50 °C Show Material materials with Relative temperature index, electrical of 50 °C | UL 746B | |||
Relative temperature index, mechanical impact | 50 °C Show Material materials with Relative temperature index, mechanical impact of 50 °C | UL 746B | |||
Relative temperature index, mechanical strength | 50 °C Show Material materials with Relative temperature index, mechanical strength of 50 °C | UL 746B | |||
Temperatura de reblandecimiento Vicat | 182 °C Show Material materials with Temperatura de reblandecimiento Vicat of 182 °C | ASTM D 1525 | Rate B/50 | |||
Inflamabilidad | UL Recognized, 94HB Flame Class Rating 2nd value | 3mm | UL 94 |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Constante dieléctrica | 23.0 °C | 3.6 [-] Show Material materials with Constante dieléctrica of 3.6 [-] | IEC 60250 | at 50/60 Hz |
Factor de disipación | 23.0 °C | 0.02 [-] Show Material materials with Factor de disipación of 0.02 [-] | IEC 60250 | at 1 MHz |
Rigidez dieléctrica | 23.0 °C | 21 kV/mm Show Material materials with Rigidez dieléctrica of 21 kV/mm | IEC 60243-1 | in oil, 3.2 mm |
Índice de seguimiento comparativo | 23.0 °C | 500 V Show Material materials with Índice de seguimiento comparativo of 500 V | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.3 - 0.7 % Show Material materials with Contracción of 0.3 - 0.7 % | SABIC method | 3.2 mm |
Contracción transversal | 23.0 °C | 0.3 - 0.7 % Show Material materials with Contracción transversal of 0.3 - 0.7 % | SABIC method |
Melt viscosity | 260.0 °C | 130 Pa·s Show Material materials with Melt viscosity of 130 Pa·s | ISO 11443 | 1500 sec⁻¹ |
Velocidad de flujo de la masa derretida | 35 g/10min Show Material materials with Velocidad de flujo de la masa derretida of 35 g/10min | ASTM D 1238 | 266°C/5.0 kg | |
Velocidad de flujo del volumen derretido | 25 cm³/10min Show Material materials with Velocidad de flujo del volumen derretido of 25 cm³/10min | ISO 1133 | 265°C/5.0 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Defense Vehicles,Enclosures,Forward Lighting,Personal Computing,Wire & cable | |
Fillers | 30% Glass Fiber | |
Processing methods | Drying Temperature: 110-120°C, Drying Time: 2-4hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 250-270°C, Nozzle Temperature: 240-260°C, Front - Zone 3 Temperature: 245-265°C, Middle - Zone 2 Temperature: 240-255°C, Rear - Zone 1 Temperature: 230-245°C, Hopper Temperature: 40-60°C, Mold Temperature: 40-100°C |