General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.23 % Show Material materials with Absorción de agua of 0.23 % | ISO 62 | 23°C, 50% RH |
Densidad | 23.0 °C | 1.21 g/cm³ Show Material materials with Densidad of 1.21 g/cm³ | ASTM D 792 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 91 % Show Material materials with Elongación of 91 % | ASTM D 638 | Type I, 50 mm/min |
Elongation at yield | 23.0 °C | 6 % Show Material materials with Elongation at yield of 6 % | ASTM D 638 | Type I, 50 mm/min |
Flexural yield strength | 23.0 °C | 83 MPa Show Material materials with Flexural yield strength of 83 MPa | ASTM D 790 | 1.3 mm/min, 50 mm span |
Impact strength, Izod notched, ASTM | -30.0 °C | 35 J/m Show Material materials with Impact strength, Izod notched, ASTM of 35 J/m | ASTM D 256 |
23.0 °C | 483 J/m Show Material materials with Impact strength, Izod notched, ASTM of 483 J/m | ASTM D 256 | |
Límite elástico | 23.0 °C | 57 MPa Show Material materials with Límite elástico of 57 MPa | ASTM D 638 | Type I, 50 mm/min |
Módulo de flexión | 23.0 °C | 1.9 GPa Show Material materials with Módulo de flexión of 1.9 GPa | ISO 178 | 2 mm/min |
Módulo elástico | 23.0 °C | 2 GPa Show Material materials with Módulo elástico of 2 GPa | ASTM D 638 | 50 mm/min |
Resistencia a la flexión | 23.0 °C | 85 MPa Show Material materials with Resistencia a la flexión of 85 MPa | ISO 178 |
Resistencia a la tracción | 23.0 °C | 45 MPa Show Material materials with Resistencia a la tracción of 45 MPa | ASTM D 638 | Type I, 50 mm/min |
Resistencia al choque, ensayo Charpy entallado | 23.0 °C | 22 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 22 kJ/m² | ISO 179/1eA |
Resistencia al choque, ensayo Izod entallado | -30.0 °C | 6 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 6 kJ/m² | ISO 180/1A |
-10.0 °C | 7 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 7 kJ/m² | ISO 180/1A | |
23.0 °C | 14 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod entallado of 14 kJ/m² | ISO 180/1A | |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 6.46E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 6.46E-5 1/K | ASTM E 831 | -40°C to 40°C |
Coeficiente de dilatación térmica transversal | 23.0 °C | 6.48E-5 1/K Show Material materials with Coeficiente de dilatación térmica transversal of 6.48E-5 1/K | ASTM E 831 | -40°C to 40°C |
Heat deflection temperature, 1.80 MPa | 95 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 95 °C | ASTM D 648 | 1.82 MPa, 3.2mm, unannealed | |
Temperatura de reblandecimiento Vicat | 112 °C Show Material materials with Temperatura de reblandecimiento Vicat of 112 °C | ASTM D 1525 | Rate B/50 |
Óptico
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 0.47 % Show Material materials with Contracción of 0.47 % | SABIC method | 3.2 mm |
Contracción transversal | 23.0 °C | 0.48 % Show Material materials with Contracción transversal of 0.48 % | SABIC method |
Velocidad de flujo de la masa derretida | 13 g/10min Show Material materials with Velocidad de flujo de la masa derretida of 13 g/10min | ASTM D 1238 | 265°C/2.16kgf | |
Velocidad de flujo del volumen derretido | 12 cm³/10min Show Material materials with Velocidad de flujo del volumen derretido of 12 cm³/10min | ISO 1133 | 265°C/2.16 kg |
Technological properties
Property | ||
---|---|---|
Application areas | Displays | |
Processing methods | Drying Temperature: 65-75°C, Drying Time: 3-5hrs, Drying Time (Cumulative): 8hrs, Maximum Moisture Content: 0.02%, Melt Temperature: 245-265°C, Nozzle Temperature: 245-265°C, Front - Zone 3 Temperature: 245-265°C, Middle - Zone 2 Temperature: 240-260°C, Rear - Zone 1 Temperature: 240-250°C, Mold Temperature: 45-60°C, Back Pressure: 0.2-0.5MPa, Screw Speed: 20-100rpm, Shot to Cylinder Size: 40-80%, Vent Depth: 0.013-0.02mm |