General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.27 % Show Material materials with Absorción de agua of 0.27 % | Sim. to ISO 62 | Immersion 24h |
Densidad | 23.0 °C | 1.42 g/cm³ Show Material materials with Densidad of 1.42 g/cm³ | ISO 1183 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.37 [-] Show Material materials with Coeficiente de Poisson of 0.37 [-] | |
Dureza Rockwell M | 23.0 °C | 90 [-] Show Material materials with Dureza Rockwell M of 90 [-] | ISO 2039-2 |
Elongación | 23.0 °C | 45 % Show Material materials with Elongación of 45 % | ISO 527-1/-2 |
Elongation at yield | 23.0 °C | 26 % Show Material materials with Elongation at yield of 26 % | ISO 527-1/-2 |
Hardness, Ball Indentation | 23.0 °C | 173 MPa Show Material materials with Hardness, Ball Indentation of 173 MPa | ISO 2039-1 |
Hardness, Rockwell R | 23.0 °C | 121 [-] Show Material materials with Hardness, Rockwell R of 121 [-] | ISO 2039-2 |
Límite elástico | 23.0 °C | 71 MPa Show Material materials with Límite elástico of 71 MPa | ISO 527-1/-2 |
Módulo de flexión | 23.0 °C | 2.8 GPa Show Material materials with Módulo de flexión of 2.8 GPa | ISO 178 |
Módulo elástico | 23.0 °C | 2.9 GPa Show Material materials with Módulo elástico of 2.9 GPa | ISO 527-1/-2 |
Resistencia a la compresión | 23.0 °C | 110 MPa Show Material materials with Resistencia a la compresión of 110 MPa | ISO 604 |
Resistencia a la flexión | 23.0 °C | 93 MPa Show Material materials with Resistencia a la flexión of 93 MPa | ISO 178 |
Resistencia al choque, ensayo Charpy entallado | -6.0 °C | 13 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 13 kJ/m² | ISO 179/1eA |
23.0 °C | 15 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 15 kJ/m² | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -6.0 °C | 425 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy no entallado of 425 kJ/m² | No Break @ 23°C, ISO 179/1eU |
Resistencia al choque, ensayo Izod no entallado | -40.0 °C | 13 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod no entallado of 13 kJ/m² | ISO 180/1A |
23.0 °C | 14 kJ/m² Show Material materials with Resistencia al choque, ensayo Izod no entallado of 14 kJ/m² | ISO 180/1A | |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Calor específico | 23.0 °C | 3000 J/(kg·K) Show Material materials with Calor específico of 3000 J/(kg·K) | of melt | ||
Coeficiente de dilatación térmica | 23.0 °C | 1E-4 1/K Show Material materials with Coeficiente de dilatación térmica of 1E-4 1/K | ISO 11359-1/-2 | -40 - 23°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 1E-4 1/K Show Material materials with Coeficiente de dilatación térmica transversal of 1E-4 1/K | ISO 11359-1/-2 | -40 - 23°C | ||
Difusividad térmica | 23.0 °C | 0 mm²/s Show Material materials with Difusividad térmica of 0 mm²/s | |||
Heat deflection temperature, 0.45 MPa | 160 °C Show Material materials with Heat deflection temperature, 0.45 MPa of 160 °C | ISO 75-1/-2 | |||
Heat deflection temperature, 1.80 MPa | 115 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 115 °C | ISO 75-1/-2 | annealed | |||
Relative temperature index, electrical | 105 °C Show Material materials with Relative temperature index, electrical of 105 °C | UL 746B | 240mil | |||
Relative temperature index, mechanical impact | 85 °C Show Material materials with Relative temperature index, mechanical impact of 85 °C | UL 746B | 240mil | |||
Relative temperature index, mechanical strength | 125 °C Show Material materials with Relative temperature index, mechanical strength of 125 °C | IEC 60216-1 | 5000 hours | |||
Temperatura de fusión | 178 °C Show Material materials with Temperatura de fusión of 178 °C | ISO 11357-1/-3 | 18°F/min | |||
Temperatura de reblandecimiento Vicat | 175 °C Show Material materials with Temperatura de reblandecimiento Vicat of 175 °C | ISO 306 | 90°F, 2 lbf | |||
Inflamabilidad | Burning Behav. at 60mil nom. thickn.: HB class, Thickness tested: 1.5 mm, UL recognition: yes -, Burning Behav. at thickness h: HB class, Thickness tested: 0.8 mm, UL recognition: yes -, Glow Wire Flammability Index, 40mil: 550 °C, Glow Wire Flammability Index, 80mil: 550 °C, Glow Wire Flammability Index, 120mil: 550 °C, Glow Wire Ignition Temperature, 30mil: 550 °C, Glow Wire Ignition Temperature, 15mil: 550 °C, Glow Wire Ignition Temperature, 40mil: 550 °C, Glow Wire Ignition Temperature, 60mil: 550 °C, Glow Wire Ignition Temperature, 80mil: 550 °C, Glow Wire Ignition Temperature, 120mil: 550 °C, FMVSS Class: B -, Burning rate, Thickness 1 mm: 40 mm/min |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Constante dieléctrica, 1 MHz | 23.0 °C | 3.8 [-] Show Material materials with Constante dieléctrica, 1 MHz of 3.8 [-] | IEC 62631-2-1 |
Constante dieléctrica, 100 Hz | 23.0 °C | 3.9 [-] Show Material materials with Constante dieléctrica, 100 Hz of 3.9 [-] | IEC 62631-2-1 |
Dissipation factor, 100Hz | 23.0 °C | 1E-3 [-] Show Material materials with Dissipation factor, 100Hz of 1E-3 [-] | IEC 62631-2-1 |
Dissipation factor, 1MHz | 23.0 °C | 5.5E-3 [-] Show Material materials with Dissipation factor, 1MHz of 5.5E-3 [-] | IEC 62631-2-1 |
Rigidez dieléctrica | 23.0 °C | 41 kV/mm Show Material materials with Rigidez dieléctrica of 41 kV/mm | IEC 60243-1 |
Surface resistivity | 23.0 °C | 3.00E+13 Ω/sq Show Material materials with Surface resistivity of 3.00E+13 Ω/sq | IEC 62631-3-2 |
Volume resistivity | 23.0 °C | 1.00E+15 Ω·cm Show Material materials with Volume resistivity of 1.00E+15 Ω·cm | min. | IEC 62631-3-1 |
Índice de seguimiento comparativo | 23.0 °C | 600 V Show Material materials with Índice de seguimiento comparativo of 600 V | IEC 60112 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 3 % Show Material materials with Contracción of 3 % | ISO 294-4 | Annealed |
Contracción transversal | 23.0 °C | 2.4 % Show Material materials with Contracción transversal of 2.4 % | ISO 294-4 | Annealed |
Velocidad de flujo de la masa derretida | 2.2 g/10min Show Material materials with Velocidad de flujo de la masa derretida of 2.2 g/10min | ISO 1133 | 190°C/2.16kg | |
Velocidad de flujo del volumen derretido | 1.9 cm³/10min Show Material materials with Velocidad de flujo del volumen derretido of 1.9 cm³/10min | ISO 1133 |
Technological properties
Property | ||
---|---|---|
Processing methods | Drying Recommended: yes, Drying Temperature: 80°C, Drying Time, Dehumidified Dryer: 2-4h, Processing Moisture Content: ≤0.2%, Melt Temperature Optimum: 215°C, Min. melt temperature: 210°C, Max. melt temperature: 220°C, Max. screw tangential speed: 0.2m/s, Mold Temperature Optimum: 90°C, Min. mold temperature: 80°C, Max. mold temperature: 100°C, Hold pressure range: 90-110MPa, Hold pressure time: 8s/mm |