General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 5.7 % Show Material materials with Absorción de agua of 5.7 % | Sim. to ISO 62 | 80mil |
Densidad | 23.0 °C | 1.39 g/cm³ Show Material materials with Densidad of 1.39 g/cm³ | ISO 1183 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.34 [-] Show Material materials with Coeficiente de Poisson of 0.34 [-] | |
Elongación | 23.0 °C | 3.5 % Show Material materials with Elongación of 3.5 % | ISO 527-1/-2 |
Módulo elástico | 23.0 °C | 11 GPa Show Material materials with Módulo elástico of 11 GPa | ISO 527-1/-2 |
Resistencia a la tracción | 23.0 °C | 200 MPa Show Material materials with Resistencia a la tracción of 200 MPa | ISO 527-1/-2 |
Resistencia al choque, ensayo Charpy entallado | -6.0 °C | 12 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 12 kJ/m² | ISO 179/1eA |
Resistencia al choque, ensayo Charpy no entallado | -6.0 °C | 90 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy no entallado of 90 kJ/m² | ISO 179/1eU |
23.0 °C | 90 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy no entallado of 90 kJ/m² | ISO 179/1eU | |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Calor específico | 23.0 °C | 1330 J/(kg·K) Show Material materials with Calor específico of 1330 J/(kg·K) | of solid | ||
Heat deflection temperature, 0.45 MPa | 260 °C Show Material materials with Heat deflection temperature, 0.45 MPa of 260 °C | ISO 75-1/-2 | |||
Heat deflection temperature, 1.80 MPa | 250 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 250 °C | ISO 75-1/-2 | |||
Relative temperature index, electrical | 130 °C Show Material materials with Relative temperature index, electrical of 130 °C | UL 746B | 120mil | |||
Relative temperature index, mechanical impact | 105 °C Show Material materials with Relative temperature index, mechanical impact of 105 °C | UL 746B | 120mil | |||
Relative temperature index, mechanical strength | 130 °C Show Material materials with Relative temperature index, mechanical strength of 130 °C | UL 746B | 120mil | |||
Temperatura de fusión | 263 °C Show Material materials with Temperatura de fusión of 263 °C | ISO 11357-1/-3 | 18°F/min | |||
Temperatura de transición del vidrio | 80 °C Show Material materials with Temperatura de transición del vidrio of 80 °C | ISO 11357-1/-2 | 18°F/min | |||
Inflamabilidad | Burning Behav. at 60mil nom. thickn.: HB class, Thickness tested: 1.5 mm, UL recognition: yes -, Burning Behav. at thickness h: HB class, Thickness tested: 0.7 mm, UL recognition: yes -, Oxygen index: 24 %, FMVSS Class: B -, Burning rate, Thickness 1 mm: <80 mm/min |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Volume resistivity | 23.0 °C | 1.00E+15 Ω·cm Show Material materials with Volume resistivity of 1.00E+15 Ω·cm | min. | IEC 62631-3-1 |
Índice de seguimiento comparativo | 23.0 °C | 600 V Show Material materials with Índice de seguimiento comparativo of 600 V | IEC 60112 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Fillers | 33% Glass Fiber | |
Processing methods | Drying Recommended: yes, Drying Temperature: 80°C, Drying Time, Dehumidified Dryer: 2-4h, Processing Moisture Content: ≤0.2%, Melt Temperature Optimum: 295°C, Min. melt temperature: 285°C, Max. melt temperature: 305°C, Max. screw tangential speed: 0.2m/s, Mold Temperature Optimum: 100°C, Min. mold temperature: 70°C, Max. mold temperature: 120°C, Hold pressure range: 50-100MPa, Hold pressure time: 3s/mm, Ejection temperature: 210°C |