Property | Temperature | Value | Comment |
---|---|---|---|
Densidad | 23.0 °C | 1.68 g/cm³ Show Material materials with Densidad of 1.68 g/cm³ | ISO 1183 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | |
Elongación | 23.0 °C | 1.9 % Show Material materials with Elongación of 1.9 % | ISO 527-1/-2 |
Módulo de flexión | 23.0 °C | 10.5 GPa Show Material materials with Módulo de flexión of 10.5 GPa | ISO 178 |
Módulo elástico | 23.0 °C | 11.3 GPa Show Material materials with Módulo elástico of 11.3 GPa | ISO 527-1/-2 |
Resistencia a la flexión | 23.0 °C | 200 MPa Show Material materials with Resistencia a la flexión of 200 MPa | ISO 178 |
Resistencia a la tracción | 23.0 °C | 130 MPa Show Material materials with Resistencia a la tracción of 130 MPa | ISO 527-1/-2 |
Resistencia al choque, ensayo Charpy entallado | -40.0 °C | 8 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 8 kJ/m² | ISO 179/1eA |
23.0 °C | 9 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 9 kJ/m² | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | -40.0 °C | 30 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy no entallado of 30 kJ/m² | ISO 179/1eU |
23.0 °C | 40 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy no entallado of 40 kJ/m² | ISO 179/1eU | |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 1.7E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 1/K | ISO 11359-1/-2 | 23 - 55°C | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 1.3E-4 1/K Show Material materials with Coeficiente de dilatación térmica transversal of 1.3E-4 1/K | ISO 11359-1/-2 | 55 - 160°C | ||
Heat deflection temperature, 0.45 MPa | 243 °C Show Material materials with Heat deflection temperature, 0.45 MPa of 243 °C | ISO 75-1/-2 | |||
Heat deflection temperature, 1.80 MPa | 220 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 220 °C | ISO 75-1/-2 | |||
Relative temperature index, electrical | 155 °C Show Material materials with Relative temperature index, electrical of 155 °C | UL 746B | 120mil | |||
Relative temperature index, mechanical impact | 155 °C Show Material materials with Relative temperature index, mechanical impact of 155 °C | UL 746B | 120mil | |||
Relative temperature index, mechanical strength | 155 °C Show Material materials with Relative temperature index, mechanical strength of 155 °C | UL 746B | 120mil | |||
Temperatura de fusión | 252 °C Show Material materials with Temperatura de fusión of 252 °C | ISO 11357-1/-3 | 18°F/min | |||
Inflamabilidad | Burning Behav. at 60mil nom. thickn.: V-0 class, Thickness tested: 1.5 mm, UL recognition: yes -, Burning Behav. at thickness h: V-0 class, Thickness tested: 0.35 mm, UL recognition: yes -, Burning Behav. 5V at thickness h: 5VA class, Thickness tested: 1.5 mm, UL recognition: yes -, Oxygen index: 33 %, Glow Wire Flammability Index, 30mil: 960 °C, Glow Wire Flammability Index, 40mil: 960 °C, Glow Wire Flammability Index, 60mil: 960 °C, Glow Wire Flammability Index, 80mil: 960 °C, Glow Wire Flammability Index, 120mil: 960 °C, Glow Wire Ignition Temperature, 30mil: 800 °C, Glow Wire Ignition Temperature, 60mil: 800 °C, Glow Wire Ignition Temperature, 80mil: 850 °C, Glow Wire Ignition Temperature, 120mil: 925 °C, FMVSS Class: DNI -, Railway classification: R23 -, Railway classification rating: HL1 - |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Constante dieléctrica, 1 MHz | 23.0 °C | 3.7 [-] Show Material materials with Constante dieléctrica, 1 MHz of 3.7 [-] | IEC 62631-2-1 |
Constante dieléctrica, 100 Hz | 23.0 °C | 4.1 [-] Show Material materials with Constante dieléctrica, 100 Hz of 4.1 [-] | IEC 62631-2-1 |
Dissipation factor, 100Hz | 23.0 °C | 0.03 [-] Show Material materials with Dissipation factor, 100Hz of 0.03 [-] | IEC 62631-2-1 |
Dissipation factor, 1MHz | 23.0 °C | 0.01 [-] Show Material materials with Dissipation factor, 1MHz of 0.01 [-] | IEC 62631-2-1 |
Surface resistivity | 23.0 °C | 1.00E+14 Ω/sq Show Material materials with Surface resistivity of 1.00E+14 Ω/sq | IEC 62631-3-2 |
Volume resistivity | 23.0 °C | 1.00E+15 Ω·cm Show Material materials with Volume resistivity of 1.00E+15 Ω·cm | min. | IEC 62631-3-1 |
Índice de seguimiento comparativo | 23.0 °C | 2 V Show Material materials with Índice de seguimiento comparativo of 2 V | UL 746A |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Fillers | 30% Glass Fiber | |
Processing methods | Drying Recommended: yes, Drying Temperature: 120°C, Drying Time, Dehumidified Dryer: 4-6h, Processing Moisture Content: ≤0.02%, Melt Temperature Optimum: 280°C, Min. melt temperature: 270°C, Max. melt temperature: 290°C, Max. screw tangential speed: 0.2m/s, Mold Temperature Optimum: 110°C, Min. mold temperature: 100°C, Max. mold temperature: 120°C, Hold pressure range: ≥80MPa, Hold pressure time: 4s/mm, Back pressure: As low as possible, Ejection temperature: 170°C |