General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 8.5 % Show Material materials with Absorción de agua of 8.5 % | Sim. to ISO 62 | 80mil |
Densidad | 23.0 °C | 1.14 g/cm³ Show Material materials with Densidad of 1.14 g/cm³ | ISO 1183 |
Mecánica
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.37 [-] Show Material materials with Coeficiente de Poisson of 0.37 [-] | |||
Elongación | 23.0 °C | 500 % Show Material materials with Elongación of 500 % | min. | ISO 527-1/-2 | ||
Elongation at yield | 23.0 °C | 4.4 % Show Material materials with Elongation at yield of 4.4 % | ISO 527-1/-2 | ||
Límite elástico | 23.0 °C | 84 MPa Show Material materials with Límite elástico of 84 MPa | ISO 527-1/-2 | ||
Módulo elástico | 23.0 °C | 3 GPa Show Material materials with Módulo elástico of 3 GPa | ISO 527-1/-2 | ||
Resistencia al choque, ensayo Charpy entallado | -6.0 °C | 6 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 6 kJ/m² | ISO 179/1eA | ||
23.0 °C | 7 kJ/m² Show Material materials with Resistencia al choque, ensayo Charpy entallado of 7 kJ/m² | ISO 179/1eA | |||
Resistencia al choque, ensayo Charpy no entallado | No Break @ 23°C, ISO 179/1eU |
Aplicaciones térmicas
Property | Temperature | Value | Comment | ||
---|---|---|---|---|---|
Coeficiente de dilatación térmica | 23.0 °C | 1E-4 1/K Show Material materials with Coeficiente de dilatación térmica of 1E-4 1/K | ISO 11359-1/-2 | ||
Coeficiente de dilatación térmica transversal | 23.0 °C | 1E-4 1/K Show Material materials with Coeficiente de dilatación térmica transversal of 1E-4 1/K | ISO 11359-1/-2 | ||
Heat deflection temperature, 0.45 MPa | 205 °C Show Material materials with Heat deflection temperature, 0.45 MPa of 205 °C | ISO 75-1/-2 | |||
Heat deflection temperature, 1.80 MPa | 74 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 74 °C | ISO 75-1/-2 | |||
Temperatura de fusión | 263 °C Show Material materials with Temperatura de fusión of 263 °C | ISO 11357-1/-3 | 18°F/min | |||
Inflamabilidad | FMVSS Class: B -, Burning rate, Thickness 1 mm: <80 mm/min |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Constante dieléctrica, 100 Hz | 23.0 °C | 3.9 [-] Show Material materials with Constante dieléctrica, 100 Hz of 3.9 [-] | IEC 62631-2-1 |
Volume resistivity | 23.0 °C | 1.00E+13 Ω·cm Show Material materials with Volume resistivity of 1.00E+13 Ω·cm | IEC 62631-3-1 |
Rheological Properties
Property | Temperature | Value | Comment |
---|---|---|---|
Contracción | 23.0 °C | 1.6 % Show Material materials with Contracción of 1.6 % | ISO 294-4, 2577 |
Technological properties
Property | ||
---|---|---|
Processing methods | Drying Recommended: yes, Drying Temperature: 80°C, Drying Time, Dehumidified Dryer: 2-4h, Processing Moisture Content: ≤0.2%, Melt Temperature Optimum: 290°C, Min. melt temperature: 280°C, Max. melt temperature: 300°C, Max. screw tangential speed: 0.4m/s, Mold Temperature Optimum: 70°C, Min. mold temperature: 50°C, Max. mold temperature: 90°C, Hold pressure range: 50-100MPa, Hold pressure time: 4s/mm, Ejection temperature: 190°C |