General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.03 % Show Material materials with Absorción de agua of 0.03 % | ma., ASTM D570, 24h |
Densidad | 23.0 °C | 0.86 g/cm³ Show Material materials with Densidad of 0.86 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 25.0 °C | 0.47 [-] Show Material materials with Coeficiente de Poisson of 0.47 [-] | |
Dureza Shore D | 23.0 °C | 55 - 65 [-] Show Material materials with Dureza Shore D of 55 - 65 [-] | ASTM D2240 |
Elongación | 23.0 °C | 275 - 320 % Show Material materials with Elongación of 275 - 320 % | ASTM D638 |
Impact strength, Izod notched, ASTM | 23.0 °C | 640 - 800 J/m Show Material materials with Impact strength, Izod notched, ASTM of 640 - 800 J/m | ASTM D256 |
Límite elástico | 23.0 °C | 16 - 18 MPa Show Material materials with Límite elástico of 16 - 18 MPa | ASTM D638 |
Módulo de flexión | 23.0 °C | 0.38 GPa Show Material materials with Módulo de flexión of 0.38 GPa | ASTM D790 |
Módulo elástico | 23.0 °C | 0.29 - 0.3 GPa Show Material materials with Módulo elástico of 0.29 - 0.3 GPa | ASTM D638 |
Resistencia a la tracción | 23.0 °C | 32 - 35 MPa Show Material materials with Resistencia a la tracción of 32 - 35 MPa | ASTM D638 |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Brittleness temperature | -18.15 °C Show Material materials with Brittleness temperature of -18.15 °C | ASTM D746 | |
Coeficiente de dilatación térmica | 23.0 °C | 6.7E-4 1/K Show Material materials with Coeficiente de dilatación térmica of 6.7E-4 1/K | for 140 to 240°C |
Conductividad térmica | 23.0 °C | 0.22 W/(m·K) Show Material materials with Conductividad térmica of 0.22 W/(m·K) | ASTM C177 |
Heat deflection temperature, 0.45 MPa | 101.85 - 112.85 °C Show Material materials with Heat deflection temperature, 0.45 MPa of 101.85 - 112.85 °C | ASTM D648 | |
Heat deflection temperature, 1.80 MPa | 53.85 - 59.85 °C Show Material materials with Heat deflection temperature, 1.80 MPa of 53.85 - 59.85 °C | ASTM D648 | |
Temperatura de transición del vidrio | 248 - 256 °C Show Material materials with Temperatura de transición del vidrio of 248 - 256 °C | DMA |
Eléctrico
Óptico
Property | Value |
---|---|
Índice de refracción | 1.51 [-] Show Material materials with Índice de refracción of 1.51 [-] |
Rheological Properties
Property | Value | Comment |
---|---|---|
Velocidad de flujo de la masa derretida | 0.4 g/10min Show Material materials with Velocidad de flujo de la masa derretida of 0.4 g/10min | ASTM D 1238(E) |
Technological properties
Property | ||
---|---|---|
Application areas | Hot water and high-pressure piping, films, adhesives, comonomer for ethylene polymers. Atactic polymer is used in sealants. |