General
Property | Temperature | Value | Comment |
---|---|---|---|
Absorción de agua | 23.0 °C | 0.4 % Show Material materials with Absorción de agua of 0.4 % | 24h |
Coeficiente de expansión higroscópica | 23.0 °C | 5E-6 % Show Material materials with Coeficiente de expansión higroscópica of 5E-6 % | |
Coeficiente de permeabilidad | 23.0 °C | 13 cm²/s Show Material materials with Coeficiente de permeabilidad of 13 cm²/s | E96 |
Índice límite de óxigeno | 23.0 °C | 25 % Show Material materials with Índice límite de óxigeno of 25 % | D2863-77 |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Elongación | 23.0 °C | 240 % Show Material materials with Elongación of 240 % | D882-67 |
Elongación transversal | 23.0 °C | 240 % Show Material materials with Elongación transversal of 240 % | D882-67 |
Resistencia a la tracción | 23.0 °C | 120 MPa Show Material materials with Resistencia a la tracción of 120 MPa | D882-67 |
Resistencia a la tracción transversal | 23.0 °C | 120 MPa Show Material materials with Resistencia a la tracción transversal of 120 MPa | D882-67 |
Aplicaciones térmicas
Property | Temperature | Value | |
---|---|---|---|
Calor específico | 23.0 °C | 1450 J/(kg·K) Show Material materials with Calor específico of 1450 J/(kg·K) | |
Coeficiente de dilatación térmica | 110.0 °C | 4E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 4E-5 1/K | |
Temperatura de transición del vidrio | 143 °C Show Material materials with Temperatura de transición del vidrio of 143 °C | ||
Temperatura máx. de funcionamiento, largo | 250 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 250 °C | ||
Inflamabilidad | UL94 VTM -1 (100 micron) |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Constante dieléctrica | 25.0 °C | 3.3 [-] Show Material materials with Constante dieléctrica of 3.3 [-] | at 50Hz, D150 |
Dissipation factor, 50Hz | 25.0 °C | 1.8E-3 [-] Show Material materials with Dissipation factor, 50Hz of 1.8E-3 [-] | D150 |
100.0 °C | 1.6E-3 [-] Show Material materials with Dissipation factor, 50Hz of 1.6E-3 [-] | D150 | |
Resistividad eléctrica | 25.0 °C | 1.00E+15 Ω·m Show Material materials with Resistividad eléctrica of 1.00E+15 Ω·m | D257 |
Rigidez dieléctrica | 23.0 °C | 128 kV/mm Show Material materials with Rigidez dieléctrica of 128 kV/mm | D194-64 |
Rheological Properties
Technological properties
Property | ||
---|---|---|
Other | “Stabar” K200 film offers an excellent combination of properties including: Intrinsic long term heat stability; Low flammability and extremely low smoke and toxic gas evolution on burning; Resistance to attack by a wide range of organic and inorganic chemicals and solvents; Low water absorption and good hydrolysis resistance at high temperatures and pressures; Resistance to radiation (X-rays, beta-rays and gamma rays) is amongst the best of thermoplastic materials; Good tear and fatigue resistance; Retention of good electrical properties over a wide temperature range. | |
Processing methods | “Stabar” K200 film can be adhesion-bonded either to itself or to other substrates, the bond strengths being dependent upon the type of adhesive and the surface preparation. “Stabar” K200 film may be fusion- bonded to itself, to reinforcements and to other substrates by application of heat and pressure. “Stabar” K200 film can be metallised by vacuum deposition and sputtering techniques, and is compatible with a range of inks and lacquers. |