Mecánica
Property | Temperature | Value |
---|---|---|
Estricción | 20.0 °C | 16 % Show Material materials with Estricción of 16 % |
650.0 °C | 27 % Show Material materials with Estricción of 27 % | |
760.0 °C | 23 % Show Material materials with Estricción of 23 % | |
Límite elástico | 20.0 °C | 700 MPa Show Material materials with Límite elástico of 700 MPa |
650.0 °C | 330 MPa Show Material materials with Límite elástico of 330 MPa | |
760.0 °C | 300 MPa Show Material materials with Límite elástico of 300 MPa | |
Resistencia a la tracción | 20.0 °C | 1070 MPa Show Material materials with Resistencia a la tracción of 1070 MPa |
650.0 °C | 640 MPa Show Material materials with Resistencia a la tracción of 640 MPa | |
760.0 °C | 510 MPa Show Material materials with Resistencia a la tracción of 510 MPa | |
Chemical properties
Property | Value |
---|---|
Carbono | 0.5 % Show Material materials with Carbono of 0.5 % |
Cromo | 20.5 % Show Material materials with Cromo of 20.5 % |
Hierro | 63.5 - 100 % Show Material materials with Hierro of 63.5 - 100 % |
Manganeso | 11.5 % Show Material materials with Manganeso of 11.5 % |
Niobio | 1 % Show Material materials with Niobio of 1 % |
Nitrógeno | 0.45 % Show Material materials with Nitrógeno of 0.45 % |
Silicona | 0.15 % Show Material materials with Silicona of 0.15 % |
Vanadio | 0.4 % Show Material materials with Vanadio of 0.4 % |
Wolframio | 2 % Show Material materials with Wolframio of 2 % |