General
Property | Value | Comment |
---|---|---|
Densidad | 7.8 g/cm³ Show Material materials with Densidad of 7.8 g/cm³ | Typical for Steel |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Steel | ||||
Elongación | 13.8 % Show Material materials with Elongación of 13.8 % | Predicted Value, A200 | ||||
15.2 % Show Material materials with Elongación of 15.2 % | Predicted Value, A80 | |||||
17.1 % Show Material materials with Elongación of 17.1 % | Predicted Value, Transverse | |||||
18.9 % Show Material materials with Elongación of 18.9 % | Predicted Value, A80 Transverse | |||||
20.4 % Show Material materials with Elongación of 20.4 % | Predicted Value, A5 | |||||
22.5 % Show Material materials with Elongación of 22.5 % | Predicted Value, A50 | |||||
20 °C | 17 % Show Material materials with Elongación of 17 % | quenched and tempered (+QT) | EN 10028-6 | Flat | ||
Estricción | 40.3 % Show Material materials with Estricción of 40.3 % | Predicted Value | ||||
44.0 % Show Material materials with Estricción of 44.0 % | Predicted Value, Transverse | |||||
Límite elástico | 297.1 MPa Show Material materials with Límite elástico of 297.1 MPa | Predicted Value, RP1 | ||||
330.5 MPa Show Material materials with Límite elástico of 330.5 MPa | Predicted Value, RP1 Transverse | |||||
438.3 MPa Show Material materials with Límite elástico of 438.3 MPa | Predicted Value, Transverse | |||||
476.2 MPa Show Material materials with Límite elástico of 476.2 MPa | Predicted Value, RP02 Transverse | |||||
524.7 MPa Show Material materials with Límite elástico of 524.7 MPa | Predicted Value, RP05 | |||||
565.8 MPa Show Material materials with Límite elástico of 565.8 MPa | Predicted Value, RP002 | |||||
20 °C | 440 MPa Show Material materials with Límite elástico of 440 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | ||
20 °C | 480 MPa Show Material materials with Límite elástico of 480 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | ||
20 °C | 500 MPa Show Material materials with Límite elástico of 500 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | ||
50 °C | 430 MPa Show Material materials with Límite elástico of 430 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
50 °C | 470 MPa Show Material materials with Límite elástico of 470 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
50 °C | 490 MPa Show Material materials with Límite elástico of 490 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
100 °C | 410 MPa Show Material materials with Límite elástico of 410 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
100 °C | 450 MPa Show Material materials with Límite elástico of 450 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
100 °C | 470 MPa Show Material materials with Límite elástico of 470 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
150 °C | 390 MPa Show Material materials with Límite elástico of 390 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
150 °C | 430 MPa Show Material materials with Límite elástico of 430 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
150 °C | 450 MPa Show Material materials with Límite elástico of 450 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
200 °C | 360 MPa Show Material materials with Límite elástico of 360 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
200 °C | 400 MPa Show Material materials with Límite elástico of 400 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
200 °C | 420 MPa Show Material materials with Límite elástico of 420 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
250 °C | 340 MPa Show Material materials with Límite elástico of 340 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
250 °C | 380 MPa Show Material materials with Límite elástico of 380 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
250 °C | 400 MPa Show Material materials with Límite elástico of 400 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
300 °C | 320 MPa Show Material materials with Límite elástico of 320 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
300 °C | 360 MPa Show Material materials with Límite elástico of 360 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
300 °C | 380 MPa Show Material materials with Límite elástico of 380 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | RP02 | |
Módulo de cizallamiento | 80.1 GPa Show Material materials with Módulo de cizallamiento of 80.1 GPa | Predicted Value | ||||
Módulo elástico | 190 - 210 GPa Show Material materials with Módulo elástico of 190 - 210 GPa | Typical for Steel | ||||
Resistencia a la tracción | 20 °C | 540 - 770 MPa Show Material materials with Resistencia a la tracción of 540 - 770 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | |
20 °C | 540 - 720 MPa Show Material materials with Resistencia a la tracción of 540 - 720 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | ||
20 °C | 590 - 770 MPa Show Material materials with Resistencia a la tracción of 590 - 770 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | ||
20 °C | 590 - 720 MPa Show Material materials with Resistencia a la tracción of 590 - 720 MPa | quenched and tempered (+QT) | EN 10028-6 | Flat | ||
Resistencia al cizallamiento | 584 MPa Show Material materials with Resistencia al cizallamiento of 584 MPa | Predicted Value |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 442.4 J/(kg·K) Show Material materials with Calor específico of 442.4 J/(kg·K) | Predicted Value |
Coeficiente de dilatación térmica | 11.96 1/K Show Material materials with Coeficiente de dilatación térmica of 11.96 1/K | Predicted Value |
Conductividad térmica | 36.37 W/(m·K) Show Material materials with Conductividad térmica of 36.37 W/(m·K) | Predicted Value |
Eléctrico
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
0.015 % Show Material materials with Azufre of 0.015 % | quenched and tempered (+QT) | EN 10028-6 | Flat | |
Boro | 0.005 % Show Material materials with Boro of 0.005 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Carbono | 0.18 % Show Material materials with Carbono of 0.18 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Circonio | 0.15 % Show Material materials with Circonio of 0.15 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Cromo | 1 % Show Material materials with Cromo of 1 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Manganeso | 1.7 % Show Material materials with Manganeso of 1.7 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Molibdeno | 0.7 % Show Material materials with Molibdeno of 0.7 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Niobio | 0.05 % Show Material materials with Niobio of 0.05 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Nitrógeno | 0.015 % Show Material materials with Nitrógeno of 0.015 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Níquel | 1.5 % Show Material materials with Níquel of 1.5 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Silicona | 0.6 % Show Material materials with Silicona of 0.6 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Titanio | 0.05 % Show Material materials with Titanio of 0.05 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Vanadio | 0.08 % Show Material materials with Vanadio of 0.08 % | quenched and tempered (+QT) | EN 10028-6 | Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |