General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 8.9 g/cm³ Show Material materials with Densidad of 8.9 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Dureza Brinell | 20.0 °C | 130 [-] Show Material materials with Dureza Brinell of 130 [-] |
Elongación | 20.0 °C | 35 - 40 % Show Material materials with Elongación of 35 - 40 % |
100.0 °C | 40 % Show Material materials with Elongación of 40 % | |
200.0 °C | 40 % Show Material materials with Elongación of 40 % | |
300.0 °C | 45 % Show Material materials with Elongación of 45 % | |
400.0 °C | 40 % Show Material materials with Elongación of 40 % | |
500.0 °C | 35 % Show Material materials with Elongación of 35 % | |
600.0 °C | 30 % Show Material materials with Elongación of 30 % | |
Elongation A100 | 20.0 °C | 20 - 30 % Show Material materials with Elongation A100 of 20 - 30 % |
Límite elástico Rp 0,2 | 20.0 °C | 100 MPa Show Material materials with Límite elástico Rp 0,2 of 100 MPa |
100.0 °C | 150 MPa Show Material materials with Límite elástico Rp 0,2 of 150 MPa | |
200.0 °C | 130 MPa Show Material materials with Límite elástico Rp 0,2 of 130 MPa | |
300.0 °C | 140 MPa Show Material materials with Límite elástico Rp 0,2 of 140 MPa | |
400.0 °C | 130 MPa Show Material materials with Límite elástico Rp 0,2 of 130 MPa | |
500.0 °C | 100 MPa Show Material materials with Límite elástico Rp 0,2 of 100 MPa | |
600.0 °C | 80 MPa Show Material materials with Límite elástico Rp 0,2 of 80 MPa | |
Límite elástico Rp 1,0 | 20.0 °C | 125 MPa Show Material materials with Límite elástico Rp 1,0 of 125 MPa |
100.0 °C | 180 MPa Show Material materials with Límite elástico Rp 1,0 of 180 MPa | |
200.0 °C | 160 MPa Show Material materials with Límite elástico Rp 1,0 of 160 MPa | |
300.0 °C | 170 MPa Show Material materials with Límite elástico Rp 1,0 of 170 MPa | |
400.0 °C | 160 MPa Show Material materials with Límite elástico Rp 1,0 of 160 MPa | |
500.0 °C | 130 MPa Show Material materials with Límite elástico Rp 1,0 of 130 MPa | |
600.0 °C | 105 MPa Show Material materials with Límite elástico Rp 1,0 of 105 MPa | |
Módulo elástico | 20.0 °C | 205 GPa Show Material materials with Módulo elástico of 205 GPa |
100.0 °C | 200 GPa Show Material materials with Módulo elástico of 200 GPa | |
200.0 °C | 196 GPa Show Material materials with Módulo elástico of 196 GPa | |
300.0 °C | 190 GPa Show Material materials with Módulo elástico of 190 GPa | |
400.0 °C | 182 GPa Show Material materials with Módulo elástico of 182 GPa | |
500.0 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | |
600.0 °C | 165 GPa Show Material materials with Módulo elástico of 165 GPa | |
700.0 °C | 153 GPa Show Material materials with Módulo elástico of 153 GPa | |
800.0 °C | 140 GPa Show Material materials with Módulo elástico of 140 GPa | |
900.0 °C | 134 GPa Show Material materials with Módulo elástico of 134 GPa | |
Resistencia a la tracción | 20.0 °C | 370 - 400 MPa Show Material materials with Resistencia a la tracción of 370 - 400 MPa |
100.0 °C | 390 MPa Show Material materials with Resistencia a la tracción of 390 MPa | |
200.0 °C | 360 MPa Show Material materials with Resistencia a la tracción of 360 MPa | |
300.0 °C | 370 MPa Show Material materials with Resistencia a la tracción of 370 MPa | |
400.0 °C | 330 MPa Show Material materials with Resistencia a la tracción of 330 MPa | |
500.0 °C | 255 MPa Show Material materials with Resistencia a la tracción of 255 MPa | |
600.0 °C | 200 MPa Show Material materials with Resistencia a la tracción of 200 MPa | |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 456 J/(kg·K) Show Material materials with Calor específico of 456 J/(kg·K) | |
100.0 °C | 475 J/(kg·K) Show Material materials with Calor específico of 475 J/(kg·K) | ||
200.0 °C | 500 J/(kg·K) Show Material materials with Calor específico of 500 J/(kg·K) | ||
300.0 °C | 570 J/(kg·K) Show Material materials with Calor específico of 570 J/(kg·K) | ||
400.0 °C | 530 J/(kg·K) Show Material materials with Calor específico of 530 J/(kg·K) | ||
500.0 °C | 525 J/(kg·K) Show Material materials with Calor específico of 525 J/(kg·K) | ||
600.0 °C | 535 J/(kg·K) Show Material materials with Calor específico of 535 J/(kg·K) | ||
700.0 °C | 550 J/(kg·K) Show Material materials with Calor específico of 550 J/(kg·K) | ||
800.0 °C | 565 J/(kg·K) Show Material materials with Calor específico of 565 J/(kg·K) | ||
900.0 °C | 580 J/(kg·K) Show Material materials with Calor específico of 580 J/(kg·K) | ||
1000.0 °C | 590 J/(kg·K) Show Material materials with Calor específico of 590 J/(kg·K) | ||
Coeficiente de dilatación térmica | 100.0 °C | 1.33E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.33E-5 1/K | |
200.0 °C | 1.39E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.39E-5 1/K | ||
300.0 °C | 1.43E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.43E-5 1/K | ||
400.0 °C | 1.48E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.48E-5 1/K | ||
500.0 °C | 1.52E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.52E-5 1/K | ||
600.0 °C | 1.56E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.56E-5 1/K | ||
700.0 °C | 1.58E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.58E-5 1/K | ||
800.0 °C | 1.62E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.62E-5 1/K | ||
900.0 °C | 1.65E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.65E-5 1/K | ||
1000.0 °C | 1.67E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.67E-5 1/K | ||
Conductividad térmica | 20.0 °C | 70.5 W/(m·K) Show Material materials with Conductividad térmica of 70.5 W/(m·K) | |
100.0 °C | 66.5 W/(m·K) Show Material materials with Conductividad térmica of 66.5 W/(m·K) | ||
200.0 °C | 61.5 W/(m·K) Show Material materials with Conductividad térmica of 61.5 W/(m·K) | ||
300.0 °C | 57 W/(m·K) Show Material materials with Conductividad térmica of 57 W/(m·K) | ||
400.0 °C | 56 W/(m·K) Show Material materials with Conductividad térmica of 56 W/(m·K) | ||
500.0 °C | 57.5 W/(m·K) Show Material materials with Conductividad térmica of 57.5 W/(m·K) | ||
600.0 °C | 60 W/(m·K) Show Material materials with Conductividad térmica of 60 W/(m·K) | ||
700.0 °C | 62 W/(m·K) Show Material materials with Conductividad térmica of 62 W/(m·K) | ||
800.0 °C | 64 W/(m·K) Show Material materials with Conductividad térmica of 64 W/(m·K) | ||
900.0 °C | 66.5 W/(m·K) Show Material materials with Conductividad térmica of 66.5 W/(m·K) | ||
1000.0 °C | 69 W/(m·K) Show Material materials with Conductividad térmica of 69 W/(m·K) | ||
Temperatura de fusión | 1400 - 1500 °C Show Material materials with Temperatura de fusión of 1400 - 1500 °C | Typical for Pure/Low Nickel Alloy |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 9E-8 Ω·m Show Material materials with Resistividad eléctrica of 9E-8 Ω·m |
100.0 °C | 1.3E-7 Ω·m Show Material materials with Resistividad eléctrica of 1.3E-7 Ω·m | |
200.0 °C | 1.9E-7 Ω·m Show Material materials with Resistividad eléctrica of 1.9E-7 Ω·m | |
300.0 °C | 2.6E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.6E-7 Ω·m | |
400.0 °C | 3.3E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.3E-7 Ω·m | |
500.0 °C | 3.7E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.7E-7 Ω·m | |
600.0 °C | 4E-7 Ω·m Show Material materials with Resistividad eléctrica of 4E-7 Ω·m | |
700.0 °C | 4.3E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.3E-7 Ω·m | |
800.0 °C | 4.5E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.5E-7 Ω·m | |
900.0 °C | 4.8E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.8E-7 Ω·m | |
1000.0 °C | 5.1E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.1E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 5E-3 % Show Material materials with Azufre of 5E-3 % |
Carbono | 0.1 % Show Material materials with Carbono of 0.1 % |
Cobalto | 1 % Show Material materials with Cobalto of 1 % |
Cobre | 0.25 % Show Material materials with Cobre of 0.25 % |
Hierro | 0.4 % Show Material materials with Hierro of 0.4 % |
Magnesio | 0.15 % Show Material materials with Magnesio of 0.15 % |
Manganeso | 0.35 % Show Material materials with Manganeso of 0.35 % |
Níquel | 98.2 % Show Material materials with Níquel of 98.2 % |
Silicona | 0.25 % Show Material materials with Silicona of 0.25 % |
Titanio | 0.1 % Show Material materials with Titanio of 0.1 % |