General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.69 g/cm³ Show Material materials with Densidad of 2.69 g/cm³ | T6 | EN 573-3, EN 755 | Rod, Tube | |
20.0 °C | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | T6 | EN 573-3 | Profile, Rod, Tube |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Dureza Brinell | 70.0 [-] Show Material materials with Dureza Brinell of 70.0 [-] | T6 | EN 573-3, EN 755 | Rod, Tube | ||
20.0 °C | 70.0 [-] Show Material materials with Dureza Brinell of 70.0 [-] | T6 | EN 573-3 | Profile, Rod, Tube | ||
Elongación | 6.0 % Show Material materials with Elongación of 6.0 % | T6 | EN 573-3, EN 755 | Rod, Tube | A50 | |
8.0 % Show Material materials with Elongación of 8.0 % | T6 | EN 573-3, EN 755 | Rod, Tube | A100 | ||
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | T6 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | T6 | EN 573-3 | Profile, Rod, Tube | ||
Módulo de cizallamiento | 26.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||||
Módulo elástico | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | T6 | EN 573-3, EN 755 | Rod, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Resistencia a la tracción | 215.0 MPa Show Material materials with Resistencia a la tracción of 215.0 MPa | T6 | EN 573-3, EN 755 | Rod, Tube | ||
20.0 °C | 215.0 MPa Show Material materials with Resistencia a la tracción of 215.0 MPa | T6 | EN 573-3 | Profile, Rod, Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 887.0 - 963.0 J/(kg·K) Show Material materials with Calor específico of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium | ||||
Coeficiente de dilatación térmica | 20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | T6 | EN 573-3, EN 755 | Rod, Tube | |
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | T6 | EN 573-3, EN 755 | Rod, Tube | ||
Conductividad térmica | 218 W/(m·K) Show Material materials with Conductividad térmica of 218 W/(m·K) | T6 | EN 573-3, EN 755 | Rod, Tube | ||
Temperatura de fusión | 620.0 - 655.0 °C Show Material materials with Temperatura de fusión of 620.0 - 655.0 °C | T6 | EN 573-3, EN 755 | Rod, Tube |
Eléctrico
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Conductividad eléctrica | 33000000.0 S/m Show Material materials with Conductividad eléctrica of 33000000.0 S/m | T6 | EN 573-3, EN 755 | Rod, Tube |
Resistividad eléctrica | 3.03e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.03e-08 Ω·m | T6 | EN 573-3, EN 755 | Rod, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.05 % Show Material materials with Cobre of 0.05 % | T6 | EN 573-3, EN 755 | Profile, Rod, Tube |
Hierro | 0.1 - 0.3 % Show Material materials with Hierro of 0.1 - 0.3 % | T6 | EN 573-3, EN 755 | Profile, Rod, Tube |
Magnesio | 0.35 - 0.6 % Show Material materials with Magnesio of 0.35 - 0.6 % | T6 | EN 573-3, EN 755 | Profile, Rod, Tube |
Manganeso | 0.05 % Show Material materials with Manganeso of 0.05 % | T6 | EN 573-3, EN 755 | Profile, Rod, Tube |
Silicona | 0.3 - 0.6 % Show Material materials with Silicona of 0.3 - 0.6 % | T6 | EN 573-3, EN 755 | Profile, Rod, Tube |
Zinc | 0.1 % Show Material materials with Zinc of 0.1 % | T6 | EN 573-3, EN 755 | Profile, Rod, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: very good, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good to acceptable / good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / -, Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) good (O) / good (O) |