General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.8 - 7.85 g/cm³ Show Material materials with Densidad of 7.8 - 7.85 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Nickel Chromium Molybdenum Steel |
Módulo de cizallamiento | 20.0 °C | 79 GPa Show Material materials with Módulo de cizallamiento of 79 GPa | |
Módulo elástico | -100.0 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | |
20.0 °C | 205 - 212 GPa Show Material materials with Módulo elástico of 205 - 212 GPa | ||
100.0 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | ||
200.0 °C | 188 - 199 GPa Show Material materials with Módulo elástico of 188 - 199 GPa | ||
300.0 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | ||
400.0 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | ||
500.0 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | ||
600.0 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | ||
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | |
20.0 °C | 460 - 461 J/(kg·K) Show Material materials with Calor específico of 460 - 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.05E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 1/K | |
20.0 °C | 1.15E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15E-5 1/K | ||
100.0 °C | 1.1E-5 - 1.21E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.1E-5 - 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36E-5 1/K | ||
500.0 °C | 1.4E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4E-5 1/K | ||
600.0 °C | 1.44E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.44E-5 1/K | ||
Conductividad térmica | 20.0 °C | 33.7 - 44 W/(m·K) Show Material materials with Conductividad térmica of 33.7 - 44 W/(m·K) | |
100.0 °C | 36.2 W/(m·K) Show Material materials with Conductividad térmica of 36.2 W/(m·K) | ||
200.0 °C | 37.8 W/(m·K) Show Material materials with Conductividad térmica of 37.8 W/(m·K) | ||
300.0 °C | 37.2 W/(m·K) Show Material materials with Conductividad térmica of 37.2 W/(m·K) | ||
400.0 °C | 35.7 W/(m·K) Show Material materials with Conductividad térmica of 35.7 W/(m·K) | ||
500.0 °C | 34 W/(m·K) Show Material materials with Conductividad térmica of 34 W/(m·K) | ||
600.0 °C | 32 W/(m·K) Show Material materials with Conductividad térmica of 32 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 9.4 mm²/s Show Material materials with Difusividad térmica of 9.4 mm²/s | |
100.0 °C | 9.4 mm²/s Show Material materials with Difusividad térmica of 9.4 mm²/s | ||
200.0 °C | 9.2 mm²/s Show Material materials with Difusividad térmica of 9.2 mm²/s | ||
300.0 °C | 8.5 mm²/s Show Material materials with Difusividad térmica of 8.5 mm²/s | ||
400.0 °C | 7.6 mm²/s Show Material materials with Difusividad térmica of 7.6 mm²/s | ||
500.0 °C | 6.6 mm²/s Show Material materials with Difusividad térmica of 6.6 mm²/s | ||
600.0 °C | 5.4 mm²/s Show Material materials with Difusividad térmica of 5.4 mm²/s | ||
Temperatura de fusión | 1382 - 1529 °C Show Material materials with Temperatura de fusión of 1382 - 1529 °C | Typical for Nickel Chromium Molybdenum Steel | |
Temperatura máx. de funcionamiento, largo | -60 - 0 °C Show Material materials with Temperatura máx. de funcionamiento, largo of -60 - 0 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.6E-7 - 3.09E-7 Ω·m Show Material materials with Resistividad eléctrica of 1.6E-7 - 3.09E-7 Ω·m |
100.0 °C | 3.54E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.54E-7 Ω·m | |
200.0 °C | 4.18E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.18E-7 Ω·m | |
300.0 °C | 5.05E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.05E-7 Ω·m | |
400.0 °C | 6.09E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.09E-7 Ω·m | |
500.0 °C | 7.27E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.27E-7 Ω·m | |
600.0 °C | 8.67E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.67E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.035 % Show Material materials with Azufre of 0.035 % |
Carbono | 0.15 - 0.2 % Show Material materials with Carbono of 0.15 - 0.2 % |
Cromo | 1.5 - 1.8 % Show Material materials with Cromo of 1.5 - 1.8 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 0.4 - 0.6 % Show Material materials with Manganeso of 0.4 - 0.6 % |
Molibdeno | 0.25 - 0.35 % Show Material materials with Molibdeno of 0.25 - 0.35 % |
Níquel | 1.4 - 1.7 % Show Material materials with Níquel of 1.4 - 1.7 % |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % |