General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.96 - 7.98 g/cm³ Show Material materials with Densidad of 7.96 - 7.98 g/cm³ |
22.0 °C | 7.96 g/cm³ Show Material materials with Densidad of 7.96 g/cm³ | |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 22.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] |
24.0 °C | 0.23 - 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.23 - 0.28 [-] | |
149.0 °C | 0.24 - 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.24 - 0.28 [-] | |
260.0 °C | 0.28 - 0.31 [-] Show Material materials with Coeficiente de Poisson of 0.28 - 0.31 [-] | |
371.0 °C | 0.33 - 0.36 [-] Show Material materials with Coeficiente de Poisson of 0.33 - 0.36 [-] | |
483.0 °C | 0.29 - 0.32 [-] Show Material materials with Coeficiente de Poisson of 0.29 - 0.32 [-] | |
593.0 °C | 0.32 [-] Show Material materials with Coeficiente de Poisson of 0.32 [-] | |
704.0 °C | 0.28 - 0.34 [-] Show Material materials with Coeficiente de Poisson of 0.28 - 0.34 [-] | |
816.0 °C | 0.22 - 0.27 [-] Show Material materials with Coeficiente de Poisson of 0.22 - 0.27 [-] | |
Elongación | 20.0 °C | 40 % Show Material materials with Elongación of 40 % |
Elongación transversal | 20.0 °C | 30 - 35 % Show Material materials with Elongación transversal of 30 - 35 % |
Límite elástico | 20.0 °C | 205 MPa Show Material materials with Límite elástico of 205 MPa |
Límite elástico Rp 0,2 | 20.0 °C | 205 MPa Show Material materials with Límite elástico Rp 0,2 of 205 MPa |
50.0 °C | 196 MPa Show Material materials with Límite elástico Rp 0,2 of 196 MPa | |
100.0 °C | 177 MPa Show Material materials with Límite elástico Rp 0,2 of 177 MPa | |
150.0 °C | 162 MPa Show Material materials with Límite elástico Rp 0,2 of 162 MPa | |
200.0 °C | 147 MPa Show Material materials with Límite elástico Rp 0,2 of 147 MPa | |
250.0 °C | 137 MPa Show Material materials with Límite elástico Rp 0,2 of 137 MPa | |
300.0 °C | 127 MPa Show Material materials with Límite elástico Rp 0,2 of 127 MPa | |
350.0 °C | 120 MPa Show Material materials with Límite elástico Rp 0,2 of 120 MPa | |
400.0 °C | 115 MPa Show Material materials with Límite elástico Rp 0,2 of 115 MPa | |
450.0 °C | 112 - 115 MPa Show Material materials with Límite elástico Rp 0,2 of 112 - 115 MPa | |
500.0 °C | 110 MPa Show Material materials with Límite elástico Rp 0,2 of 110 MPa | |
550.0 °C | 108 MPa Show Material materials with Límite elástico Rp 0,2 of 108 MPa | |
Límite elástico Rp 1,0 | 20.0 °C | 240 MPa Show Material materials with Límite elástico Rp 1,0 of 240 MPa |
50.0 °C | 230 MPa Show Material materials with Límite elástico Rp 1,0 of 230 MPa | |
100.0 °C | 211 MPa Show Material materials with Límite elástico Rp 1,0 of 211 MPa | |
150.0 °C | 191 MPa Show Material materials with Límite elástico Rp 1,0 of 191 MPa | |
200.0 °C | 177 MPa Show Material materials with Límite elástico Rp 1,0 of 177 MPa | |
250.0 °C | 167 MPa Show Material materials with Límite elástico Rp 1,0 of 167 MPa | |
300.0 °C | 156 MPa Show Material materials with Límite elástico Rp 1,0 of 156 MPa | |
350.0 °C | 150 MPa Show Material materials with Límite elástico Rp 1,0 of 150 MPa | |
400.0 °C | 144 MPa Show Material materials with Límite elástico Rp 1,0 of 144 MPa | |
450.0 °C | 141 MPa Show Material materials with Límite elástico Rp 1,0 of 141 MPa | |
500.0 °C | 139 MPa Show Material materials with Límite elástico Rp 1,0 of 139 MPa | |
550.0 °C | 137 MPa Show Material materials with Límite elástico Rp 1,0 of 137 MPa | |
Límite elástico transversal | 20.0 °C | 205 MPa Show Material materials with Límite elástico transversal of 205 MPa |
Límite elástico transversal Rp 0,2 | 20.0 °C | 205 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 205 MPa |
Límite elástico transversal Rp 1,0 | 20.0 °C | 240 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 240 MPa |
Módulo de cizallamiento | 22.0 °C | 75.8 GPa Show Material materials with Módulo de cizallamiento of 75.8 GPa |
24.0 °C | 77.2 - 78.6 GPa Show Material materials with Módulo de cizallamiento of 77.2 - 78.6 GPa | |
149.0 °C | 74.5 GPa Show Material materials with Módulo de cizallamiento of 74.5 GPa | |
260.0 °C | 69.6 - 71 GPa Show Material materials with Módulo de cizallamiento of 69.6 - 71 GPa | |
371.0 °C | 64.1 - 67.6 GPa Show Material materials with Módulo de cizallamiento of 64.1 - 67.6 GPa | |
483.0 °C | 62.1 - 64.1 GPa Show Material materials with Módulo de cizallamiento of 62.1 - 64.1 GPa | |
593.0 °C | 57.9 - 60 GPa Show Material materials with Módulo de cizallamiento of 57.9 - 60 GPa | |
704.0 °C | 54.5 - 55.9 GPa Show Material materials with Módulo de cizallamiento of 54.5 - 55.9 GPa | |
816.0 °C | 51 - 52.4 GPa Show Material materials with Módulo de cizallamiento of 51 - 52.4 GPa | |
Módulo elástico | -100.0 °C | 206 GPa Show Material materials with Módulo elástico of 206 GPa |
20.0 °C | 196 - 200 GPa Show Material materials with Módulo elástico of 196 - 200 GPa | |
22.0 °C | 196.2 GPa Show Material materials with Módulo elástico of 196.2 GPa | |
24.0 °C | 193.1 - 197.9 GPa Show Material materials with Módulo elástico of 193.1 - 197.9 GPa | |
100.0 °C | 190 - 194 GPa Show Material materials with Módulo elástico of 190 - 194 GPa | |
149.0 °C | 184.8 - 190.3 GPa Show Material materials with Módulo elástico of 184.8 - 190.3 GPa | |
200.0 °C | 182 - 186 GPa Show Material materials with Módulo elástico of 182 - 186 GPa | |
260.0 °C | 182 - 182.7 GPa Show Material materials with Módulo elástico of 182 - 182.7 GPa | |
300.0 °C | 174 - 179 GPa Show Material materials with Módulo elástico of 174 - 179 GPa | |
371.0 °C | 174.4 - 179.3 GPa Show Material materials with Módulo elástico of 174.4 - 179.3 GPa | |
400.0 °C | 166 - 172 GPa Show Material materials with Módulo elástico of 166 - 172 GPa | |
483.0 °C | 163.4 - 165.5 GPa Show Material materials with Módulo elástico of 163.4 - 165.5 GPa | |
500.0 °C | 158 - 165 GPa Show Material materials with Módulo elástico of 158 - 165 GPa | |
593.0 °C | 153.4 - 157.9 GPa Show Material materials with Módulo elástico of 153.4 - 157.9 GPa | |
600.0 °C | 150 GPa Show Material materials with Módulo elástico of 150 GPa | |
700.0 °C | 142 GPa Show Material materials with Módulo elástico of 142 GPa | |
704.0 °C | 143.4 - 146.2 GPa Show Material materials with Módulo elástico of 143.4 - 146.2 GPa | |
800.0 °C | 134 GPa Show Material materials with Módulo elástico of 134 GPa | |
816.0 °C | 124.1 - 133.1 GPa Show Material materials with Módulo elástico of 124.1 - 133.1 GPa | |
900.0 °C | 127 GPa Show Material materials with Módulo elástico of 127 GPa | |
1000.0 °C | 120 GPa Show Material materials with Módulo elástico of 120 GPa | |
Resistencia a la tracción | 20.0 °C | 510 - 710 MPa Show Material materials with Resistencia a la tracción of 510 - 710 MPa |
Resistencia a la tracción transversal | 20.0 °C | 510 - 710 MPa Show Material materials with Resistencia a la tracción transversal of 510 - 710 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 440 J/(kg·K) Show Material materials with Calor específico of 440 J/(kg·K) | |
20.0 °C | 472 - 500 J/(kg·K) Show Material materials with Calor específico of 472 - 500 J/(kg·K) | ||
100.0 °C | 487 J/(kg·K) Show Material materials with Calor específico of 487 J/(kg·K) | ||
200.0 °C | 503 J/(kg·K) Show Material materials with Calor específico of 503 J/(kg·K) | ||
300.0 °C | 512 J/(kg·K) Show Material materials with Calor específico of 512 J/(kg·K) | ||
400.0 °C | 520 J/(kg·K) Show Material materials with Calor específico of 520 J/(kg·K) | ||
500.0 °C | 530 J/(kg·K) Show Material materials with Calor específico of 530 J/(kg·K) | ||
600.0 °C | 541 J/(kg·K) Show Material materials with Calor específico of 541 J/(kg·K) | ||
700.0 °C | 551 J/(kg·K) Show Material materials with Calor específico of 551 J/(kg·K) | ||
800.0 °C | 559 J/(kg·K) Show Material materials with Calor específico of 559 J/(kg·K) | ||
900.0 °C | 565 J/(kg·K) Show Material materials with Calor específico of 565 J/(kg·K) | ||
1000.0 °C | 571 J/(kg·K) Show Material materials with Calor específico of 571 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | |
20.0 °C | 1.61E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.61E-5 1/K | ||
100.0 °C | 1.65E-5 - 1.67E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.65E-5 - 1.67E-5 1/K | ||
200.0 °C | 1.72E-5 - 1.75E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.72E-5 - 1.75E-5 1/K | ||
300.0 °C | 1.75E-5 - 1.77E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.75E-5 - 1.77E-5 1/K | ||
400.0 °C | 1.81E-5 - 1.85E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.81E-5 - 1.85E-5 1/K | ||
500.0 °C | 1.84E-5 - 1.85E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.84E-5 - 1.85E-5 1/K | ||
600.0 °C | 1.88E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.88E-5 1/K | ||
700.0 °C | 1.91E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.91E-5 1/K | ||
800.0 °C | 1.94E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.94E-5 1/K | ||
900.0 °C | 1.97E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.97E-5 1/K | ||
1000.0 °C | 2E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 2E-5 1/K | ||
Conductividad térmica | 20.0 °C | 13.3 - 15 W/(m·K) Show Material materials with Conductividad térmica of 13.3 - 15 W/(m·K) | |
100.0 °C | 14.9 W/(m·K) Show Material materials with Conductividad térmica of 14.9 W/(m·K) | ||
200.0 °C | 16.5 W/(m·K) Show Material materials with Conductividad térmica of 16.5 W/(m·K) | ||
300.0 °C | 18.1 W/(m·K) Show Material materials with Conductividad térmica of 18.1 W/(m·K) | ||
400.0 °C | 19.5 W/(m·K) Show Material materials with Conductividad térmica of 19.5 W/(m·K) | ||
500.0 °C | 21 W/(m·K) Show Material materials with Conductividad térmica of 21 W/(m·K) | ||
600.0 °C | 22.4 W/(m·K) Show Material materials with Conductividad térmica of 22.4 W/(m·K) | ||
700.0 °C | 23.8 W/(m·K) Show Material materials with Conductividad térmica of 23.8 W/(m·K) | ||
800.0 °C | 25.2 W/(m·K) Show Material materials with Conductividad térmica of 25.2 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 3.5 mm²/s Show Material materials with Difusividad térmica of 3.5 mm²/s | |
100.0 °C | 3.8 mm²/s Show Material materials with Difusividad térmica of 3.8 mm²/s | ||
200.0 °C | 4 mm²/s Show Material materials with Difusividad térmica of 4 mm²/s | ||
300.0 °C | 4.3 mm²/s Show Material materials with Difusividad térmica of 4.3 mm²/s | ||
400.0 °C | 4.5 mm²/s Show Material materials with Difusividad térmica of 4.5 mm²/s | ||
500.0 °C | 4.7 mm²/s Show Material materials with Difusividad térmica of 4.7 mm²/s | ||
600.0 °C | 4.8 mm²/s Show Material materials with Difusividad térmica of 4.8 mm²/s | ||
700.0 °C | 5.1 mm²/s Show Material materials with Difusividad térmica of 5.1 mm²/s | ||
800.0 °C | 5.4 mm²/s Show Material materials with Difusividad térmica of 5.4 mm²/s | ||
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel | |
Temperatura máx. de funcionamiento, largo | 0 - 300 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 300 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 7.5E-7 - 7.91E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.5E-7 - 7.91E-7 Ω·m |
100.0 °C | 8.45E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.45E-7 Ω·m | |
200.0 °C | 9.19E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.19E-7 Ω·m | |
300.0 °C | 9.77E-7 Ω·m Show Material materials with Resistividad eléctrica of 9.77E-7 Ω·m | |
400.0 °C | 1.03E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.03E-6 Ω·m | |
500.0 °C | 1.08E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.08E-6 Ω·m | |
600.0 °C | 1.12E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.12E-6 Ω·m | |
700.0 °C | 1.15E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.15E-6 Ω·m | |
800.0 °C | 1.18E-6 Ω·m Show Material materials with Resistividad eléctrica of 1.18E-6 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 - 0.03 % Show Material materials with Azufre of 0.015 - 0.03 % |
Carbono | 0.03 - 0.07 % Show Material materials with Carbono of 0.03 - 0.07 % |
Cromo | 16.5 - 18.5 % Show Material materials with Cromo of 16.5 - 18.5 % |
Fósforo | 0.05 - 0.45 % Show Material materials with Fósforo of 0.05 - 0.45 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Molibdeno | 2 - 2.5 % Show Material materials with Molibdeno of 2 - 2.5 % |
Nitrógeno | 0.11 % Show Material materials with Nitrógeno of 0.11 % |
Níquel | 10 - 13.5 % Show Material materials with Níquel of 10 - 13.5 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |