General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3 | Coil, Sheet, Foil, Flat, Plate |
Medidas
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | H22 | EN 573-3 | Foil, Flat, Plate | |
Dureza Brinell | 36.0 [-] Show Material materials with Dureza Brinell of 36.0 [-] | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 36.0 [-] Show Material materials with Dureza Brinell of 36.0 [-] | H22 | EN 573-3 | Flat | ||
Dureza Brinell (HBW) | 36 [-] Show Material materials with Dureza Brinell (HBW) of 36 [-] | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
Elongación | 5.0 % Show Material materials with Elongación of 5.0 % | H22 | EN 573-3, EN 546 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | |
6.0 % Show Material materials with Elongación of 6.0 % | H22 | EN 573-3, EN 485, EN 546 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
6.0 - 8.0 % Show Material materials with Elongación of 6.0 - 8.0 % | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | A50 | ||
7.0 % Show Material materials with Elongación of 7.0 % | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
8.0 % Show Material materials with Elongación of 8.0 % | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
9.0 % Show Material materials with Elongación of 9.0 % | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
10.0 % Show Material materials with Elongación of 10.0 % | H22 | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
11.0 % Show Material materials with Elongación of 11.0 % | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | H22 | EN 573-3 | Plate | A50 | |
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | H22 | EN 573-3 | Plate | A50 | |
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | H22 | EN 573-3 | Plate | A50 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 5.0 % Show Material materials with Elongación of 5.0 % | H22 | EN 573-3 | Foil, Plate | A50 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H22 | EN 573-3 | Foil, Plate, Flat | A50 | |
20.0 °C | 6.0 % Show Material materials with Elongación of 6.0 % | H22 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | H22 | EN 573-3 | Foil, Flat | A50 | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | H22 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 7.0 % Show Material materials with Elongación of 7.0 % | H22 | EN 573-3 | Plate | ||
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | H22 | EN 573-3 | Foil, Flat | A50 | |
20.0 °C | 8.0 % Show Material materials with Elongación of 8.0 % | H22 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | H22 | EN 573-3 | Foil, Flat | A50 | |
20.0 °C | 9.0 % Show Material materials with Elongación of 9.0 % | H22 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H22 | EN 573-3 | Foil | A50 | |
20.0 °C | 10.0 % Show Material materials with Elongación of 10.0 % | H22 | EN 573-3 | Plate | ||
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | H22 | EN 573-3 | Foil, Flat | A50 | |
20.0 °C | 11.0 % Show Material materials with Elongación of 11.0 % | H22 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | H22 | EN 573-3 | Foil | A100 | |
20.0 °C | 14.0 % Show Material materials with Elongación of 14.0 % | H22 | EN 573-3 | Foil | A50 | |
Límite elástico | 75.0 MPa Show Material materials with Límite elástico of 75.0 MPa | H22 | EN 573-3, EN 485, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP02 | |
75 MPa Show Material materials with Límite elástico of 75 MPa | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |||
20.0 °C | 75.0 MPa Show Material materials with Límite elástico of 75.0 MPa | H22 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 75.0 MPa Show Material materials with Límite elástico of 75.0 MPa | H22 | EN 573-3 | Foil, Plate, Flat | RP02 | |
20.0 °C | 80.0 MPa Show Material materials with Límite elástico of 80.0 MPa | H22 | EN 573-3 | Foil | RP02 | |
20.0 °C | 110.0 MPa Show Material materials with Límite elástico of 110.0 MPa | H22 | EN 573-3 | Plate | RP02 | |
Módulo de cizallamiento | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
26.5 GPa Show Material materials with Módulo de cizallamiento of 26.5 GPa | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |||
20.0 °C | 24.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.5 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 24.0 - 26.1 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.1 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 26.1 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.1 - 26.5 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
Módulo elástico | -270.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3 | Coil, Sheet, Foil, Flat, Plate | |
69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 69.0 - 70.0 GPa Show Material materials with Módulo elástico of 69.0 - 70.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 69.0 - 69.5 GPa Show Material materials with Módulo elástico of 69.0 - 69.5 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 69.5 - 70.0 GPa Show Material materials with Módulo elástico of 69.5 - 70.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3 | Coil, Sheet, Foil, Flat, Plate | ||
50.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
100.0 °C | 68.0 GPa Show Material materials with Módulo elástico of 68.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
150.0 °C | 66.0 GPa Show Material materials with Módulo elástico of 66.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
200.0 °C | 63.0 GPa Show Material materials with Módulo elástico of 63.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
250.0 °C | 57.0 GPa Show Material materials with Módulo elástico of 57.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
300.0 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | H22 | EN 573-3 | Foil, Flat, Plate | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Resistencia a la tracción | 20.0 °C | 115.0 - 155.0 MPa Show Material materials with Resistencia a la tracción of 115.0 - 155.0 MPa | H22 | EN 573-3, EN 485, EN 546, EN 683, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Coil, Sheet, Flat | |
20.0 °C | 115.0 - 175.0 MPa Show Material materials with Resistencia a la tracción of 115.0 - 175.0 MPa | H22 | EN 573-3 | Plate | ||
20.0 °C | 115.0 - 195.0 MPa Show Material materials with Resistencia a la tracción of 115.0 - 195.0 MPa | H22 | EN 573-3 | Plate | ||
20.0 °C | 115.0 - 155.0 MPa Show Material materials with Resistencia a la tracción of 115.0 - 155.0 MPa | H22 | EN 573-3 | Flat | Transverse | |
20.0 °C | 120.0 - 160.0 MPa Show Material materials with Resistencia a la tracción of 120.0 - 160.0 MPa | H22 | EN 573-3 | Foil | ||
20.0 °C | 140.0 - 175.0 MPa Show Material materials with Resistencia a la tracción of 140.0 - 175.0 MPa | H22 | EN 573-3 | Plate | ||
20.0 °C | 140.0 - 195.0 MPa Show Material materials with Resistencia a la tracción of 140.0 - 195.0 MPa | H22 | EN 573-3 | Plate | ||
Ángulo de flexión a 180° | 1.0 °/t Show Material materials with Ángulo de flexión a 180° of 1.0 °/t | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
1.5 °/t Show Material materials with Ángulo de flexión a 180° of 1.5 °/t | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |||
Ángulo de flexión a 90° | 0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
0.5 °/t Show Material materials with Ángulo de flexión a 90° of 0.5 °/t | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |||
1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 892.0 - 893.0 J/(kg·K) Show Material materials with Calor específico of 892.0 - 893.0 J/(kg·K) | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 892.0 J/(kg·K) Show Material materials with Calor específico of 892.0 J/(kg·K) | H22 | EN 573-3 | Foil, Flat, Plate | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H22 | EN 573-3 | Foil, Flat, Plate | ||
Coeficiente de dilatación térmica | 20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
100 °C | 0.000025 1/K Show Material materials with Coeficiente de dilatación térmica of 0.000025 1/K | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | 20-100°C | |
Conductividad térmica | 176 W/(m·K) Show Material materials with Conductividad térmica of 176 W/(m·K) | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 200.0 W/(m·K) | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20.0 °C | 160.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 W/(m·K) | H22 | EN 573-3 | Foil, Flat, Plate | ||
Temperatura de fusión | 645.0 - 655.0 °C Show Material materials with Temperatura de fusión of 645.0 - 655.0 °C | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 22000000.0 - 28000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 28000000.0 S/m | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat |
20.0 °C | 22000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 29000000.0 S/m | H22 | EN 573-3 | Foil, Flat, Plate | |
Resistividad eléctrica | 3.57e-08 - 4.55e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.57e-08 - 4.55e-08 Ω·m | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
4.3e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.3e-08 Ω·m | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
20.0 °C | 3.4e-08 - 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.1e-08 Ω·m | H22 | EN 573-3 | Foil, Flat, Plate | |
20.0 °C | 3.4e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.5e-08 Ω·m | H22 | EN 573-3 | Foil, Flat, Plate | |
20.0 °C | 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 Ω·m | H22 | EN 573-3 | Foil, Flat, Plate | |
20.0 °C | 4.1e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 - 4.5e-08 Ω·m | H22 | EN 573-3 | Foil, Flat, Plate |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H22 | EN 573-3, EN 485, EN 546, EN 683 | Foil, Flat, Plate, Strip, Sheet, Bar, Rod, Tube |
0.1 % Show Material materials with Cobre of 0.1 % | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | H22 | EN 573-3, EN 485, EN 546, EN 683 | Foil, Flat, Plate, Strip, Sheet, Bar, Rod, Tube |
0.1 % Show Material materials with Cromo of 0.1 % | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | H22 | EN 573-3 | Foil, Flat, Plate |
0.70 % Show Material materials with Hierro of 0.70 % | H22 | EN 573-3, EN 485, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
0.7 % Show Material materials with Hierro of 0.7 % | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Magnesio | 0.3 % Show Material materials with Magnesio of 0.3 % | H22 | EN 573-3, EN 485, EN 546, EN 683 | Foil, Flat, Plate, Strip, Sheet, Bar, Rod, Tube |
0.3 % Show Material materials with Magnesio of 0.3 % | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Manganeso | 0.9 - 1.5 % Show Material materials with Manganeso of 0.9 - 1.5 % | H22 | EN 573-3, EN 485, EN 546, EN 683, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Foil, Flat, Plate, Strip, Sheet, Bar, Rod, Tube, Coil, Sheet |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | H22 | EN 573-3, EN 485, EN 546, EN 683 | Foil, Flat, Plate, Strip, Sheet, Bar, Rod, Tube |
0.5 % Show Material materials with Silicona of 0.5 % | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H22 | EN 573-3, EN 485, EN 546, EN 683 | Foil, Flat, Plate, Strip, Sheet, Bar, Rod, Tube |
0.2 % Show Material materials with Zinc of 0.2 % | H22 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing Quality; Lithography; Heat exchangers: Fins, Heat exchangers; Tubes: Flexible tube, Pipes; Cosmetics: Cosmetics pieces; Semi-rigid and corrugated: Smooth wall; Components: Automotive fins, Heat exchangers | |
Brazing | hard brazing (with flux/ without flux): very good to good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: good, weathering: very good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): good, Deep drawing / upsetting (Condition) very good (O) / very good (H12) |