General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.8 g/cm³ Show Material materials with Densidad of 7.8 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.27 [-] Show Material materials with Coeficiente de Poisson of 0.27 [-] |
100.0 °C | 0.27 [-] Show Material materials with Coeficiente de Poisson of 0.27 [-] | |
200.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] | |
300.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] | |
400.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] | |
500.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] | |
Dureza Brinell | 20.0 °C | 241 [-] Show Material materials with Dureza Brinell of 241 [-] |
Módulo de cizallamiento | 20.0 °C | 82.04 GPa Show Material materials with Módulo de cizallamiento of 82.04 GPa |
100.0 °C | 80.18 GPa Show Material materials with Módulo de cizallamiento of 80.18 GPa | |
200.0 °C | 77.56 GPa Show Material materials with Módulo de cizallamiento of 77.56 GPa | |
300.0 °C | 74.62 GPa Show Material materials with Módulo de cizallamiento of 74.62 GPa | |
400.0 °C | 71.22 GPa Show Material materials with Módulo de cizallamiento of 71.22 GPa | |
500.0 °C | 67.36 GPa Show Material materials with Módulo de cizallamiento of 67.36 GPa | |
Módulo elástico | -100.0 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa |
20.0 °C | 208.26 - 212 GPa Show Material materials with Módulo elástico of 208.26 - 212 GPa | |
100.0 °C | 203.78 - 207 GPa Show Material materials with Módulo elástico of 203.78 - 207 GPa | |
200.0 °C | 198.06 - 199 GPa Show Material materials with Módulo elástico of 198.06 - 199 GPa | |
300.0 °C | 190.8 - 192 GPa Show Material materials with Módulo elástico of 190.8 - 192 GPa | |
400.0 °C | 182.61 - 184 GPa Show Material materials with Módulo elástico of 182.61 - 184 GPa | |
500.0 °C | 173.04 - 175 GPa Show Material materials with Módulo elástico of 173.04 - 175 GPa | |
600.0 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19E-5 1/K | ||
100.0 °C | 1.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25E-5 1/K | ||
200.0 °C | 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3E-5 1/K | ||
300.0 °C | 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36E-5 1/K | ||
400.0 °C | 1.41E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41E-5 1/K | ||
500.0 °C | 1.45E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45E-5 1/K | ||
600.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | ||
Conductividad térmica | 20.0 °C | 41.7 W/(m·K) Show Material materials with Conductividad térmica of 41.7 W/(m·K) | |
100.0 °C | 43.4 W/(m·K) Show Material materials with Conductividad térmica of 43.4 W/(m·K) | ||
200.0 °C | 43.2 W/(m·K) Show Material materials with Conductividad térmica of 43.2 W/(m·K) | ||
300.0 °C | 41.4 W/(m·K) Show Material materials with Conductividad térmica of 41.4 W/(m·K) | ||
400.0 °C | 39.1 W/(m·K) Show Material materials with Conductividad térmica of 39.1 W/(m·K) | ||
500.0 °C | 36.7 W/(m·K) Show Material materials with Conductividad térmica of 36.7 W/(m·K) | ||
600.0 °C | 34.1 W/(m·K) Show Material materials with Conductividad térmica of 34.1 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 11.6 mm²/s Show Material materials with Difusividad térmica of 11.6 mm²/s | |
100.0 °C | 11.3 mm²/s Show Material materials with Difusividad térmica of 11.3 mm²/s | ||
200.0 °C | 10.5 mm²/s Show Material materials with Difusividad térmica of 10.5 mm²/s | ||
300.0 °C | 9.5 mm²/s Show Material materials with Difusividad térmica of 9.5 mm²/s | ||
400.0 °C | 8.3 mm²/s Show Material materials with Difusividad térmica of 8.3 mm²/s | ||
500.0 °C | 7.1 mm²/s Show Material materials with Difusividad térmica of 7.1 mm²/s | ||
600.0 °C | 5.8 mm²/s Show Material materials with Difusividad térmica of 5.8 mm²/s | ||
Temperatura de fusión | 1289 - 1478 °C Show Material materials with Temperatura de fusión of 1289 - 1478 °C | Typical for High Carbon Steel | |
Temperatura máx. de funcionamiento | 500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel | |
Temperatura máx. de funcionamiento, largo | -25 - 0 °C Show Material materials with Temperatura máx. de funcionamiento, largo of -25 - 0 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 2.5E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.5E-7 Ω·m |
100.0 °C | 2.95E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.95E-7 Ω·m | |
200.0 °C | 3.65E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.65E-7 Ω·m | |
300.0 °C | 4.53E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.53E-7 Ω·m | |
400.0 °C | 5.56E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.56E-7 Ω·m | |
500.0 °C | 6.74E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.74E-7 Ω·m | |
600.0 °C | 8.13E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.13E-7 Ω·m | |
Chemical properties
Property | Value |
---|---|
Azufre | 0.045 % Show Material materials with Azufre of 0.045 % |
Carbono | 0.57 - 0.65 % Show Material materials with Carbono of 0.57 - 0.65 % |
Fósforo | 0.05 % Show Material materials with Fósforo of 0.05 % |
Manganeso | 0.6 - 0.9 % Show Material materials with Manganeso of 0.6 - 0.9 % |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % |