General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.85 g/cm³ Show Material materials with Densidad of 7.85 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.28 [-] Show Material materials with Coeficiente de Poisson of 0.28 [-] | |
Elongación | 20.0 °C | 6 % Show Material materials with Elongación of 6 % | |
Módulo de cizallamiento | 23.0 °C | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel |
Módulo elástico | -100.0 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | |
20.0 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | ||
100.0 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | ||
200.0 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | ||
300.0 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | ||
400.0 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | ||
500.0 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | ||
600.0 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | ||
Resistencia a la tracción | 20.0 °C | 490 MPa Show Material materials with Resistencia a la tracción of 490 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | |
20.0 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19E-5 1/K | ||
100.0 °C | 1.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25E-5 1/K | ||
200.0 °C | 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3E-5 1/K | ||
300.0 °C | 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36E-5 1/K | ||
400.0 °C | 1.41E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41E-5 1/K | ||
500.0 °C | 1.45E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45E-5 1/K | ||
600.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | ||
Conductividad térmica | 20.0 °C | 56.9 W/(m·K) Show Material materials with Conductividad térmica of 56.9 W/(m·K) | |
100.0 °C | 56.4 W/(m·K) Show Material materials with Conductividad térmica of 56.4 W/(m·K) | ||
200.0 °C | 53.5 W/(m·K) Show Material materials with Conductividad térmica of 53.5 W/(m·K) | ||
300.0 °C | 49.4 W/(m·K) Show Material materials with Conductividad térmica of 49.4 W/(m·K) | ||
400.0 °C | 45.2 W/(m·K) Show Material materials with Conductividad térmica of 45.2 W/(m·K) | ||
500.0 °C | 41.3 W/(m·K) Show Material materials with Conductividad térmica of 41.3 W/(m·K) | ||
600.0 °C | 37.6 W/(m·K) Show Material materials with Conductividad térmica of 37.6 W/(m·K) | ||
Difusividad térmica | 20.0 °C | 15.7 mm²/s Show Material materials with Difusividad térmica of 15.7 mm²/s | |
100.0 °C | 14.5 mm²/s Show Material materials with Difusividad térmica of 14.5 mm²/s | ||
200.0 °C | 12.9 mm²/s Show Material materials with Difusividad térmica of 12.9 mm²/s | ||
300.0 °C | 11.2 mm²/s Show Material materials with Difusividad térmica of 11.2 mm²/s | ||
400.0 °C | 9.6 mm²/s Show Material materials with Difusividad térmica of 9.6 mm²/s | ||
500.0 °C | 7.9 mm²/s Show Material materials with Difusividad térmica of 7.9 mm²/s | ||
600.0 °C | 6.3 mm²/s Show Material materials with Difusividad térmica of 6.3 mm²/s | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | |
Temperatura máx. de funcionamiento | 500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel | |
Temperatura máx. de funcionamiento, largo | 0 - 300 °C Show Material materials with Temperatura máx. de funcionamiento, largo of 0 - 300 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.83E-7 Ω·m Show Material materials with Resistividad eléctrica of 1.83E-7 Ω·m |
100.0 °C | 2.27E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.27E-7 Ω·m | |
200.0 °C | 2.95E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.95E-7 Ω·m | |
300.0 °C | 3.8E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.8E-7 Ω·m | |
400.0 °C | 4.81E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.81E-7 Ω·m | |
500.0 °C | 5.99E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.99E-7 Ω·m | |
600.0 °C | 7.38E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.38E-7 Ω·m | |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value |
---|---|
Azufre | 0.025 % Show Material materials with Azufre of 0.025 % |
Carbono | 0.17 % Show Material materials with Carbono of 0.17 % |
Fósforo | 0.03 % Show Material materials with Fósforo of 0.03 % |
Manganeso | 0.7 % Show Material materials with Manganeso of 0.7 % |
Silicona | 0.3 % Show Material materials with Silicona of 0.3 % |