General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.84 g/cm³ Show Material materials with Densidad of 7.84 g/cm³ | normalized or normalized formed (+N) | EN 10028-3 | Flat |
20 °C | 7.84 - 7.85 g/cm³ Show Material materials with Densidad of 7.84 - 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 7.85 g/cm³ Show Material materials with Densidad of 7.85 g/cm³ | normalized or normalized formed (+N) | EN 10028-3 | Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Low Carbon Steel | ||||
Dureza Brinell | 241 [-] Show Material materials with Dureza Brinell of 241 [-] | Predicted Value, Transverse | ||||
Elongación | 18.0 % Show Material materials with Elongación of 18.0 % | Predicted Value, A80 Transverse | ||||
18.6 % Show Material materials with Elongación of 18.6 % | Predicted Value, A200 | |||||
19.8 % Show Material materials with Elongación of 19.8 % | Predicted Value, A80 | |||||
21.2 % Show Material materials with Elongación of 21.2 % | Predicted Value, A5 | |||||
22.6 % Show Material materials with Elongación of 22.6 % | Predicted Value, Transverse | |||||
24.9 % Show Material materials with Elongación of 24.9 % | Predicted Value, A50 | |||||
20 °C | 22 % Show Material materials with Elongación of 22 % | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | ||
20 °C | 23 % Show Material materials with Elongación of 23 % | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 24 % Show Material materials with Elongación of 24 % | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Estricción | 41.3 % Show Material materials with Estricción of 41.3 % | Predicted Value | ||||
42.7 % Show Material materials with Estricción of 42.7 % | Predicted Value, Transverse | |||||
Límite elástico | 258 MPa Show Material materials with Límite elástico of 258 MPa | Predicted Value, RP1 | ||||
315.3 MPa Show Material materials with Límite elástico of 315.3 MPa | Predicted Value, RP1 Transverse | |||||
326.9 MPa Show Material materials with Límite elástico of 326.9 MPa | Predicted Value, Transverse | |||||
395.2 MPa Show Material materials with Límite elástico of 395.2 MPa | Predicted Value, RP05 | |||||
451.4 MPa Show Material materials with Límite elástico of 451.4 MPa | Predicted Value, RP02 Transverse | |||||
461.3 MPa Show Material materials with Límite elástico of 461.3 MPa | Predicted Value, RP002 | |||||
20 °C | 215 MPa Show Material materials with Límite elástico of 215 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | ||
20 °C | 225 MPa Show Material materials with Límite elástico of 225 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 235 MPa Show Material materials with Límite elástico of 235 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 255 MPa Show Material materials with Límite elástico of 255 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 265 MPa Show Material materials with Límite elástico of 265 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 275 MPa Show Material materials with Límite elástico of 275 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
50 °C | 205 MPa Show Material materials with Límite elástico of 205 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
50 °C | 208 MPa Show Material materials with Límite elástico of 208 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 218 MPa Show Material materials with Límite elástico of 218 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 227 MPa Show Material materials with Límite elástico of 227 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 247 MPa Show Material materials with Límite elástico of 247 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 256 MPa Show Material materials with Límite elástico of 256 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 266 MPa Show Material materials with Límite elástico of 266 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 196 MPa Show Material materials with Límite elástico of 196 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
100 °C | 205 MPa Show Material materials with Límite elástico of 205 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
100 °C | 214 MPa Show Material materials with Límite elástico of 214 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 232 MPa Show Material materials with Límite elástico of 232 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 241 MPa Show Material materials with Límite elástico of 241 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 250 MPa Show Material materials with Límite elástico of 250 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 176 MPa Show Material materials with Límite elástico of 176 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
150 °C | 181 MPa Show Material materials with Límite elástico of 181 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 190 MPa Show Material materials with Límite elástico of 190 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 198 MPa Show Material materials with Límite elástico of 198 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 215 MPa Show Material materials with Límite elástico of 215 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 223 MPa Show Material materials with Límite elástico of 223 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 232 MPa Show Material materials with Límite elástico of 232 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 157 MPa Show Material materials with Límite elástico of 157 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
200 °C | 167 MPa Show Material materials with Límite elástico of 167 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 174 MPa Show Material materials with Límite elástico of 174 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 182 MPa Show Material materials with Límite elástico of 182 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 197 MPa Show Material materials with Límite elástico of 197 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 205 MPa Show Material materials with Límite elástico of 205 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
200 °C | 213 MPa Show Material materials with Límite elástico of 213 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 137 MPa Show Material materials with Límite elástico of 137 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
250 °C | 153 MPa Show Material materials with Límite elástico of 153 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 160 MPa Show Material materials with Límite elástico of 160 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 167 MPa Show Material materials with Límite elástico of 167 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 181 MPa Show Material materials with Límite elástico of 181 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 188 MPa Show Material materials with Límite elástico of 188 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 195 MPa Show Material materials with Límite elástico of 195 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 108 MPa Show Material materials with Límite elástico of 108 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
300 °C | 140 MPa Show Material materials with Límite elástico of 140 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 147 MPa Show Material materials with Límite elástico of 147 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 153 MPa Show Material materials with Límite elástico of 153 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 166 MPa Show Material materials with Límite elástico of 166 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 173 MPa Show Material materials with Límite elástico of 173 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 179 MPa Show Material materials with Límite elástico of 179 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 88 MPa Show Material materials with Límite elástico of 88 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
350 °C | 130 MPa Show Material materials with Límite elástico of 130 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 136 MPa Show Material materials with Límite elástico of 136 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 142 MPa Show Material materials with Límite elástico of 142 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 154 MPa Show Material materials with Límite elástico of 154 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 160 MPa Show Material materials with Límite elástico of 160 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 166 MPa Show Material materials with Límite elástico of 166 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 68 MPa Show Material materials with Límite elástico of 68 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
400 °C | 122 MPa Show Material materials with Límite elástico of 122 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 128 MPa Show Material materials with Límite elástico of 128 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 133 MPa Show Material materials with Límite elástico of 133 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 145 MPa Show Material materials with Límite elástico of 145 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 150 MPa Show Material materials with Límite elástico of 150 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 156 MPa Show Material materials with Límite elástico of 156 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Resistencia a la tracción | 20 °C | 340 - 470 MPa Show Material materials with Resistencia a la tracción of 340 - 470 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | |
20 °C | 350 - 510 MPa Show Material materials with Resistencia a la tracción of 350 - 510 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 350 - 490 MPa Show Material materials with Resistencia a la tracción of 350 - 490 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 350 - 480 MPa Show Material materials with Resistencia a la tracción of 350 - 480 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 350 - 470 MPa Show Material materials with Resistencia a la tracción of 350 - 470 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 360 - 510 MPa Show Material materials with Resistencia a la tracción of 360 - 510 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 360 - 490 MPa Show Material materials with Resistencia a la tracción of 360 - 490 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 360 - 480 MPa Show Material materials with Resistencia a la tracción of 360 - 480 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 360 - 470 MPa Show Material materials with Resistencia a la tracción of 360 - 470 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 370 - 510 MPa Show Material materials with Resistencia a la tracción of 370 - 510 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 370 - 490 MPa Show Material materials with Resistencia a la tracción of 370 - 490 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 370 - 480 MPa Show Material materials with Resistencia a la tracción of 370 - 480 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 370 - 470 MPa Show Material materials with Resistencia a la tracción of 370 - 470 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 390 - 510 MPa Show Material materials with Resistencia a la tracción of 390 - 510 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 390 - 490 MPa Show Material materials with Resistencia a la tracción of 390 - 490 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 390 - 480 MPa Show Material materials with Resistencia a la tracción of 390 - 480 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 390 - 470 MPa Show Material materials with Resistencia a la tracción of 390 - 470 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Resistencia al cizallamiento | 535.6 MPa Show Material materials with Resistencia al cizallamiento of 535.6 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 430 J/(kg·K) Show Material materials with Calor específico of 430 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 430 - 461 J/(kg·K) Show Material materials with Calor específico of 430 - 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Coeficiente de dilatación térmica | -100 °C | 1.08e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 1.19e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Conductividad térmica | -100 °C | 52.6 W/(m·K) Show Material materials with Conductividad térmica of 52.6 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 53.4 - 54 W/(m·K) Show Material materials with Conductividad térmica of 53.4 - 54 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 53.4 W/(m·K) Show Material materials with Conductividad térmica of 53.4 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 54 W/(m·K) Show Material materials with Conductividad térmica of 54 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 53.3 W/(m·K) Show Material materials with Conductividad térmica of 53.3 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 50.1 W/(m·K) Show Material materials with Conductividad térmica of 50.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 46.9 W/(m·K) Show Material materials with Conductividad térmica of 46.9 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 43.2 W/(m·K) Show Material materials with Conductividad térmica of 43.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 39.5 W/(m·K) Show Material materials with Conductividad térmica of 39.5 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 36.1 W/(m·K) Show Material materials with Conductividad térmica of 36.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Difusividad térmica | -100 °C | 18 mm²/s Show Material materials with Difusividad térmica of 18 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 14.8 mm²/s Show Material materials with Difusividad térmica of 14.8 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 13.7 mm²/s Show Material materials with Difusividad térmica of 13.7 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 12.1 mm²/s Show Material materials with Difusividad térmica of 12.1 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 10.6 mm²/s Show Material materials with Difusividad térmica of 10.6 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 9.2 mm²/s Show Material materials with Difusividad térmica of 9.2 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 7.6 mm²/s Show Material materials with Difusividad térmica of 7.6 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 6.1 mm²/s Show Material materials with Difusividad térmica of 6.1 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Temperatura máx. de funcionamiento | -20 - 400 °C Show Material materials with Temperatura máx. de funcionamiento of -20 - 400 °C | normalized or normalized formed (+N) | EN 10028-3 | Flat | Long | |
400 °C Show Material materials with Temperatura máx. de funcionamiento of 400 °C | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | Long | ||
500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 5 S/m Show Material materials with Conductividad eléctrica of 5 S/m | Predicted Value | ||||
Resistividad eléctrica | -100 °C | 1.3e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.3e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 1.95e-07 - 2e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.95e-07 - 2e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 1.95e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.95e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 2e-07 Ω·m Show Material materials with Resistividad eléctrica of 2e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 2.4e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.4e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 3.15e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.15e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 4e-07 Ω·m Show Material materials with Resistividad eléctrica of 4e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 5.03e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.03e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 6.26e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.26e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 7.68e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.68e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 0.02 % Show Material materials with Aluminio of 0.02 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Azufre | 0.01 % Show Material materials with Azufre of 0.01 % | normalized or normalized formed (+N) | EN 10028-3 | Flat |
0.015 % Show Material materials with Azufre of 0.015 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | |
Carbono | 0.16 % Show Material materials with Carbono of 0.16 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Cobre | 0.3 % Show Material materials with Cobre of 0.3 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Cromo | 0.3 % Show Material materials with Cromo of 0.3 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Manganeso | 0.8 - 1.5 % Show Material materials with Manganeso of 0.8 - 1.5 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Molibdeno | 0.08 % Show Material materials with Molibdeno of 0.08 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Niobio | 0.05 % Show Material materials with Niobio of 0.05 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Nitrógeno | 0.012 % Show Material materials with Nitrógeno of 0.012 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Níquel | 0.5 % Show Material materials with Níquel of 0.5 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Titanio | 0.03 % Show Material materials with Titanio of 0.03 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Vanadio | 0.05 % Show Material materials with Vanadio of 0.05 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |