General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.84 g/cm³ Show Material materials with Densidad of 7.84 g/cm³ | normalized or normalized formed (+N) | EN 10028-3 | Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Steel | ||||
Dureza Brinell | 246 [-] Show Material materials with Dureza Brinell of 246 [-] | Predicted Value, Transverse | ||||
Elongación | 13.9 % Show Material materials with Elongación of 13.9 % | Predicted Value, A200 | ||||
15.0 % Show Material materials with Elongación of 15.0 % | Predicted Value, A80 | |||||
16.5 % Show Material materials with Elongación of 16.5 % | Predicted Value, A80 Transverse | |||||
17.0 % Show Material materials with Elongación of 17.0 % | Predicted Value, Transverse | |||||
19.9 % Show Material materials with Elongación of 19.9 % | Predicted Value, A50 | |||||
20.9 % Show Material materials with Elongación of 20.9 % | Predicted Value, A5 | |||||
20 °C | 16 % Show Material materials with Elongación of 16 % | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | ||
20 °C | 17 % Show Material materials with Elongación of 17 % | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Estricción | 38.6 % Show Material materials with Estricción of 38.6 % | Predicted Value | ||||
44 % Show Material materials with Estricción of 44 % | Predicted Value, Transverse | |||||
Límite elástico | 274.1 MPa Show Material materials with Límite elástico of 274.1 MPa | Predicted Value, RP1 | ||||
314.5 MPa Show Material materials with Límite elástico of 314.5 MPa | Predicted Value, RP1 Transverse | |||||
433.6 MPa Show Material materials with Límite elástico of 433.6 MPa | Predicted Value, Transverse | |||||
464.1 MPa Show Material materials with Límite elástico of 464.1 MPa | Predicted Value, RP02 Transverse | |||||
505.2 MPa Show Material materials with Límite elástico of 505.2 MPa | Predicted Value, RP002 | |||||
520.9 MPa Show Material materials with Límite elástico of 520.9 MPa | Predicted Value, RP05 | |||||
20 °C | 370 MPa Show Material materials with Límite elástico of 370 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | ||
20 °C | 380 MPa Show Material materials with Límite elástico of 380 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 400 MPa Show Material materials with Límite elástico of 400 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 430 MPa Show Material materials with Límite elástico of 430 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 445 MPa Show Material materials with Límite elástico of 445 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 460 MPa Show Material materials with Límite elástico of 460 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
50 °C | 358 MPa Show Material materials with Límite elástico of 358 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 360 MPa Show Material materials with Límite elástico of 360 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
50 °C | 368 MPa Show Material materials with Límite elástico of 368 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 387 MPa Show Material materials with Límite elástico of 387 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 416 MPa Show Material materials with Límite elástico of 416 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 430 MPa Show Material materials with Límite elástico of 430 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
50 °C | 445 MPa Show Material materials with Límite elástico of 445 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 337 MPa Show Material materials with Límite elástico of 337 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 343 MPa Show Material materials with Límite elástico of 343 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
100 °C | 346 MPa Show Material materials with Límite elástico of 346 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 364 MPa Show Material materials with Límite elástico of 364 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 391 MPa Show Material materials with Límite elástico of 391 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 405 MPa Show Material materials with Límite elástico of 405 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
100 °C | 419 MPa Show Material materials with Límite elástico of 419 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 312 MPa Show Material materials with Límite elástico of 312 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 314 MPa Show Material materials with Límite elástico of 314 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
150 °C | 320 MPa Show Material materials with Límite elástico of 320 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 337 MPa Show Material materials with Límite elástico of 337 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 362 MPa Show Material materials with Límite elástico of 362 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 375 MPa Show Material materials with Límite elástico of 375 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
150 °C | 388 MPa Show Material materials with Límite elástico of 388 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 287 MPa Show Material materials with Límite elástico of 287 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 294 MPa Show Material materials with Límite elástico of 294 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
200 °C | 295 MPa Show Material materials with Límite elástico of 295 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 310 MPa Show Material materials with Límite elástico of 310 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 333 MPa Show Material materials with Límite elástico of 333 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 345 MPa Show Material materials with Límite elástico of 345 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
200 °C | 356 MPa Show Material materials with Límite elástico of 356 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 263 MPa Show Material materials with Límite elástico of 263 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 265 MPa Show Material materials with Límite elástico of 265 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
250 °C | 270 MPa Show Material materials with Límite elástico of 270 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 284 MPa Show Material materials with Límite elástico of 284 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 305 MPa Show Material materials with Límite elástico of 305 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 316 MPa Show Material materials with Límite elástico of 316 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
250 °C | 326 MPa Show Material materials with Límite elástico of 326 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 241 MPa Show Material materials with Límite elástico of 241 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 245 MPa Show Material materials with Límite elástico of 245 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
300 °C | 248 MPa Show Material materials with Límite elástico of 248 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 261 MPa Show Material materials with Límite elástico of 261 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 281 MPa Show Material materials with Límite elástico of 281 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 290 MPa Show Material materials with Límite elástico of 290 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
300 °C | 300 MPa Show Material materials with Límite elástico of 300 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 216 MPa Show Material materials with Límite elástico of 216 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
350 °C | 224 MPa Show Material materials with Límite elástico of 224 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 230 MPa Show Material materials with Límite elástico of 230 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 242 MPa Show Material materials with Límite elástico of 242 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 260 MPa Show Material materials with Límite elástico of 260 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 269 MPa Show Material materials with Límite elástico of 269 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
350 °C | 278 MPa Show Material materials with Límite elástico of 278 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 186 MPa Show Material materials with Límite elástico of 186 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | RP02 | |
400 °C | 210 MPa Show Material materials with Límite elástico of 210 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 216 MPa Show Material materials with Límite elástico of 216 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet | RP02 | |
400 °C | 227 MPa Show Material materials with Límite elástico of 227 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 244 MPa Show Material materials with Límite elástico of 244 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 253 MPa Show Material materials with Límite elástico of 253 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
400 °C | 261 MPa Show Material materials with Límite elástico of 261 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | RP02 | |
Módulo de cizallamiento | 80.3 GPa Show Material materials with Módulo de cizallamiento of 80.3 GPa | Predicted Value | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 210 GPa Show Material materials with Módulo elástico of 210 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 210 - 212 GPa Show Material materials with Módulo elástico of 210 - 212 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Resistencia a la tracción | 20 °C | 510 - 690 MPa Show Material materials with Resistencia a la tracción of 510 - 690 MPa | normalized or normalized formed (+N) | EN 10028-3 | Sheet, Flat | |
20 °C | 510 - 720 MPa Show Material materials with Resistencia a la tracción of 510 - 720 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 510 - 710 MPa Show Material materials with Resistencia a la tracción of 510 - 710 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 520 - 720 MPa Show Material materials with Resistencia a la tracción of 520 - 720 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 520 - 710 MPa Show Material materials with Resistencia a la tracción of 520 - 710 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 520 - 690 MPa Show Material materials with Resistencia a la tracción of 520 - 690 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 540 - 720 MPa Show Material materials with Resistencia a la tracción of 540 - 720 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 540 - 710 MPa Show Material materials with Resistencia a la tracción of 540 - 710 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 540 - 690 MPa Show Material materials with Resistencia a la tracción of 540 - 690 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 570 - 720 MPa Show Material materials with Resistencia a la tracción of 570 - 720 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 570 - 710 MPa Show Material materials with Resistencia a la tracción of 570 - 710 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 570 - 690 MPa Show Material materials with Resistencia a la tracción of 570 - 690 MPa | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
Resistencia al cizallamiento | 509.3 MPa Show Material materials with Resistencia al cizallamiento of 509.3 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat |
20 °C | 430 J/(kg·K) Show Material materials with Calor específico of 430 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 430 - 461 J/(kg·K) Show Material materials with Calor específico of 430 - 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
Coeficiente de dilatación térmica | -100 °C | 1.05e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat |
20 °C | 1.15e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
100 °C | 1.21e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
200 °C | 1.27e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
300 °C | 1.32e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
400 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
500 °C | 1.4e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.4e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
600 °C | 1.44e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.44e-05 1/K | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
Conductividad térmica | -100 °C | 34.7 W/(m·K) Show Material materials with Conductividad térmica of 34.7 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat |
20 °C | 39.7 - 40 W/(m·K) Show Material materials with Conductividad térmica of 39.7 - 40 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 39.7 W/(m·K) Show Material materials with Conductividad térmica of 39.7 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 40 W/(m·K) Show Material materials with Conductividad térmica of 40 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
100 °C | 40.9 W/(m·K) Show Material materials with Conductividad térmica of 40.9 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
200 °C | 41 W/(m·K) Show Material materials with Conductividad térmica of 41 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
300 °C | 39.9 W/(m·K) Show Material materials with Conductividad térmica of 39.9 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
400 °C | 38.2 W/(m·K) Show Material materials with Conductividad térmica of 38.2 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
500 °C | 36.1 W/(m·K) Show Material materials with Conductividad térmica of 36.1 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
600 °C | 33.8 W/(m·K) Show Material materials with Conductividad térmica of 33.8 W/(m·K) | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
Difusividad térmica | -100 °C | 11.9 mm²/s Show Material materials with Difusividad térmica of 11.9 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat |
20 °C | 11 mm²/s Show Material materials with Difusividad térmica of 11 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
100 °C | 10.5 mm²/s Show Material materials with Difusividad térmica of 10.5 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
200 °C | 9.9 mm²/s Show Material materials with Difusividad térmica of 9.9 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
300 °C | 9.1 mm²/s Show Material materials with Difusividad térmica of 9.1 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
400 °C | 8.1 mm²/s Show Material materials with Difusividad térmica of 8.1 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
500 °C | 6.9 mm²/s Show Material materials with Difusividad térmica of 6.9 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
600 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | normalized or normalized formed (+N) | EN 10028-3 | Flat |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 5 S/m Show Material materials with Conductividad eléctrica of 5 S/m | Predicted Value | ||||
Resistividad eléctrica | -100 °C | 1.97e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.97e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | |
20 °C | 2.6e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.6e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 2.6e-07 - 2.62e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.6e-07 - 2.62e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
20 °C | 2.62e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.62e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
100 °C | 3.13e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.13e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
200 °C | 3.85e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.85e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
300 °C | 4.7e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.7e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
400 °C | 5.69e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.69e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
500 °C | 6.85e-07 Ω·m Show Material materials with Resistividad eléctrica of 6.85e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat | ||
600 °C | 8.2e-07 Ω·m Show Material materials with Resistividad eléctrica of 8.2e-07 Ω·m | normalized or normalized formed (+N) | EN 10028-3 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 0.02 % Show Material materials with Aluminio of 0.02 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Carbono | 0.2 % Show Material materials with Carbono of 0.2 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Cobre | 0.7 % Show Material materials with Cobre of 0.7 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Cromo | 0.3 % Show Material materials with Cromo of 0.3 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Manganeso | 1.1 - 1.7 % Show Material materials with Manganeso of 1.1 - 1.7 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Molibdeno | 0.1 % Show Material materials with Molibdeno of 0.1 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Niobio | 0.05 % Show Material materials with Niobio of 0.05 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Nitrógeno | 0.025 % Show Material materials with Nitrógeno of 0.025 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Níquel | 0.8 % Show Material materials with Níquel of 0.8 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Silicona | 0.6 % Show Material materials with Silicona of 0.6 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Titanio | 0.03 % Show Material materials with Titanio of 0.03 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Vanadio | 0.2 % Show Material materials with Vanadio of 0.2 % | normalized or normalized formed (+N) | EN 10028-3 | Flat, Sheet |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |