General
Property | Value | Comment |
---|---|---|
Densidad | 7.8 g/cm³ Show Material materials with Densidad of 7.8 g/cm³ | Typical for Steel |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Steel | ||||
Dureza Brinell | 251 [-] Show Material materials with Dureza Brinell of 251 [-] | Predicted Value, Transverse | ||||
Elongación | 15.6 % Show Material materials with Elongación of 15.6 % | Predicted Value, A80 | ||||
15.7 % Show Material materials with Elongación of 15.7 % | Predicted Value, A200 | |||||
17.5 % Show Material materials with Elongación of 17.5 % | Predicted Value, Transverse | |||||
18.3 % Show Material materials with Elongación of 18.3 % | Predicted Value, A80 Transverse | |||||
20.9 % Show Material materials with Elongación of 20.9 % | Predicted Value, A5 | |||||
23.4 % Show Material materials with Elongación of 23.4 % | Predicted Value, A50 | |||||
20 °C | 16 % Show Material materials with Elongación of 16 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 17 % Show Material materials with Elongación of 17 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Estricción | 43.8 % Show Material materials with Estricción of 43.8 % | Predicted Value, Transverse | ||||
51.5 % Show Material materials with Estricción of 51.5 % | Predicted Value | |||||
Límite elástico | 259.8 MPa Show Material materials with Límite elástico of 259.8 MPa | Predicted Value, RP1 | ||||
319.7 MPa Show Material materials with Límite elástico of 319.7 MPa | Predicted Value, RP1 Transverse | |||||
408.3 MPa Show Material materials with Límite elástico of 408.3 MPa | Predicted Value, Transverse | |||||
429.3 MPa Show Material materials with Límite elástico of 429.3 MPa | Predicted Value, RP02 | |||||
469.9 MPa Show Material materials with Límite elástico of 469.9 MPa | Predicted Value, RP02 Transverse | |||||
506.8 MPa Show Material materials with Límite elástico of 506.8 MPa | Predicted Value, RP002 | |||||
531.5 MPa Show Material materials with Límite elástico of 531.5 MPa | Predicted Value, RP05 | |||||
20 °C | 370 MPa Show Material materials with Límite elástico of 370 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 380 MPa Show Material materials with Límite elástico of 380 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 400 MPa Show Material materials with Límite elástico of 400 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 410 MPa Show Material materials with Límite elástico of 410 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 430 MPa Show Material materials with Límite elástico of 430 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 440 MPa Show Material materials with Límite elástico of 440 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 460 MPa Show Material materials with Límite elástico of 460 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
Módulo de cizallamiento | 80.2 GPa Show Material materials with Módulo de cizallamiento of 80.2 GPa | Predicted Value | ||||
Módulo elástico | 190 - 210 GPa Show Material materials with Módulo elástico of 190 - 210 GPa | Typical for Steel | ||||
Resistencia a la tracción | 20 °C | 510 - 720 MPa Show Material materials with Resistencia a la tracción of 510 - 720 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | |
20 °C | 510 - 700 MPa Show Material materials with Resistencia a la tracción of 510 - 700 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 510 - 690 MPa Show Material materials with Resistencia a la tracción of 510 - 690 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 520 - 690 MPa Show Material materials with Resistencia a la tracción of 520 - 690 MPa | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Flat | ||
20 °C | 530 - 720 MPa Show Material materials with Resistencia a la tracción of 530 - 720 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 530 - 700 MPa Show Material materials with Resistencia a la tracción of 530 - 700 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 530 - 690 MPa Show Material materials with Resistencia a la tracción of 530 - 690 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 550 - 720 MPa Show Material materials with Resistencia a la tracción of 550 - 720 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar | ||
20 °C | 550 - 700 MPa Show Material materials with Resistencia a la tracción of 550 - 700 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
20 °C | 550 - 690 MPa Show Material materials with Resistencia a la tracción of 550 - 690 MPa | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | ||
Resistencia al cizallamiento | 527.9 MPa Show Material materials with Resistencia al cizallamiento of 527.9 MPa | Predicted Value |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 454.3 J/(kg·K) Show Material materials with Calor específico of 454.3 J/(kg·K) | Predicted Value |
Coeficiente de dilatación térmica | 11.83 1/K Show Material materials with Coeficiente de dilatación térmica of 11.83 1/K | Predicted Value |
Conductividad térmica | 38.26 W/(m·K) Show Material materials with Conductividad térmica of 38.26 W/(m·K) | Predicted Value |
Eléctrico
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 0.02 % Show Material materials with Aluminio of 0.02 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Azufre | 0.02 % Show Material materials with Azufre of 0.02 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.025 % Show Material materials with Azufre of 0.025 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat | |
Carbono | 0.2 % Show Material materials with Carbono of 0.2 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Cobre | 0.55 % Show Material materials with Cobre of 0.55 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.7 % Show Material materials with Cobre of 0.7 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat | |
Cromo | 0.3 % Show Material materials with Cromo of 0.3 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Fósforo | 0.025 % Show Material materials with Fósforo of 0.025 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.03 % Show Material materials with Fósforo of 0.03 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat | |
Manganeso | 1 - 1.7 % Show Material materials with Manganeso of 1 - 1.7 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Molibdeno | 0.1 % Show Material materials with Molibdeno of 0.1 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Niobio | 0.05 % Show Material materials with Niobio of 0.05 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat |
0.2 % Show Material materials with Niobio of 0.2 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | |
Nitrógeno | 0.025 % Show Material materials with Nitrógeno of 0.025 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Níquel | 0.8 % Show Material materials with Níquel of 0.8 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Silicona | 0.6 % Show Material materials with Silicona of 0.6 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire, Bar |
Titanio | 0.03 % Show Material materials with Titanio of 0.03 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat |
0.05 % Show Material materials with Titanio of 0.05 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire | |
Vanadio | 0.05 % Show Material materials with Vanadio of 0.05 % | normalized or normalized formed (+N) | EN 10025-3, EN 10113-2 | Strip, Sheet, Flat, Rod, Wire |
0.2 % Show Material materials with Vanadio of 0.2 % | normalized or normalized formed (+N) | EN 10113-2, EN 10025-3 | Sheet, Strip, Bar, Flat |
Technological properties
Property | ||
---|---|---|
Supplier Disclaimer | The given information is a rough description and some properties can depend on various factors such as product thickness. Please contact the supplier or refer to the related norm or standard for further information. |