General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.83 - 7.85 g/cm³ Show Material materials with Densidad of 7.83 - 7.85 g/cm³ |
Mecánica
Property | Temperature | Value |
---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] |
100.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
200.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | |
300.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
400.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | |
500.0 °C | 0.31 [-] Show Material materials with Coeficiente de Poisson of 0.31 [-] | |
Elongación | 20.0 °C | 20 - 22 % Show Material materials with Elongación of 20 - 22 % |
Estricción | 20.0 °C | 40 - 45 % Show Material materials with Estricción of 40 - 45 % |
Límite elástico | 20.0 °C | 300 - 350 MPa Show Material materials with Límite elástico of 300 - 350 MPa |
Módulo de cizallamiento | 20.0 °C | 81 - 82.19 GPa Show Material materials with Módulo de cizallamiento of 81 - 82.19 GPa |
100.0 °C | 80.03 GPa Show Material materials with Módulo de cizallamiento of 80.03 GPa | |
200.0 °C | 76.94 GPa Show Material materials with Módulo de cizallamiento of 76.94 GPa | |
300.0 °C | 73.69 GPa Show Material materials with Módulo de cizallamiento of 73.69 GPa | |
400.0 °C | 70.14 GPa Show Material materials with Módulo de cizallamiento of 70.14 GPa | |
500.0 °C | 66.12 GPa Show Material materials with Módulo de cizallamiento of 66.12 GPa | |
Módulo elástico | -100.0 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa |
20.0 °C | 210 - 212 GPa Show Material materials with Módulo elástico of 210 - 212 GPa | |
100.0 °C | 205 - 207 GPa Show Material materials with Módulo elástico of 205 - 207 GPa | |
200.0 °C | 195 - 199 GPa Show Material materials with Módulo elástico of 195 - 199 GPa | |
300.0 °C | 185 - 192 GPa Show Material materials with Módulo elástico of 185 - 192 GPa | |
400.0 °C | 175 - 184 GPa Show Material materials with Módulo elástico of 175 - 184 GPa | |
500.0 °C | 172.88 - 175 GPa Show Material materials with Módulo elástico of 172.88 - 175 GPa | |
600.0 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | |
Resistencia a la tracción | 20.0 °C | 500 - 700 MPa Show Material materials with Resistencia a la tracción of 500 - 700 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | -100.0 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | |
20.0 °C | 460 - 461 J/(kg·K) Show Material materials with Calor específico of 460 - 461 J/(kg·K) | ||
100.0 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | ||
200.0 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | ||
300.0 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | ||
400.0 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | ||
500.0 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | ||
600.0 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08E-5 1/K | |
20.0 °C | 1.19E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19E-5 1/K | ||
100.0 °C | 1.11E-5 - 1.25E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.11E-5 - 1.25E-5 1/K | ||
200.0 °C | 1.21E-5 - 1.3E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 - 1.3E-5 1/K | ||
300.0 °C | 1.29E-5 - 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.29E-5 - 1.36E-5 1/K | ||
400.0 °C | 1.35E-5 - 1.41E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.35E-5 - 1.41E-5 1/K | ||
500.0 °C | 1.45E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45E-5 1/K | ||
600.0 °C | 1.49E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49E-5 1/K | ||
Conductividad térmica | -100.0 °C | 37.6 W/(m·K) Show Material materials with Conductividad térmica of 37.6 W/(m·K) | |
20.0 °C | 42.2 - 52 W/(m·K) Show Material materials with Conductividad térmica of 42.2 - 52 W/(m·K) | ||
100.0 °C | 43.2 - 51 W/(m·K) Show Material materials with Conductividad térmica of 43.2 - 51 W/(m·K) | ||
200.0 °C | 42.9 - 49 W/(m·K) Show Material materials with Conductividad térmica of 42.9 - 49 W/(m·K) | ||
300.0 °C | 41.2 - 46 W/(m·K) Show Material materials with Conductividad térmica of 41.2 - 46 W/(m·K) | ||
400.0 °C | 39.1 W/(m·K) Show Material materials with Conductividad térmica of 39.1 W/(m·K) | ||
500.0 °C | 36.6 W/(m·K) Show Material materials with Conductividad térmica of 36.6 W/(m·K) | ||
600.0 °C | 34.1 W/(m·K) Show Material materials with Conductividad térmica of 34.1 W/(m·K) | ||
Difusividad térmica | -100.0 °C | 12.9 mm²/s Show Material materials with Difusividad térmica of 12.9 mm²/s | |
20.0 °C | 11.7 mm²/s Show Material materials with Difusividad térmica of 11.7 mm²/s | ||
100.0 °C | 11.2 mm²/s Show Material materials with Difusividad térmica of 11.2 mm²/s | ||
200.0 °C | 10.3 mm²/s Show Material materials with Difusividad térmica of 10.3 mm²/s | ||
300.0 °C | 9.4 mm²/s Show Material materials with Difusividad térmica of 9.4 mm²/s | ||
400.0 °C | 8.3 mm²/s Show Material materials with Difusividad térmica of 8.3 mm²/s | ||
500.0 °C | 7.1 mm²/s Show Material materials with Difusividad térmica of 7.1 mm²/s | ||
600.0 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | |
Temperatura máx. de funcionamiento | 500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel | |
Temperatura máx. de funcionamiento, largo | -25 - 0 °C Show Material materials with Temperatura máx. de funcionamiento, largo of -25 - 0 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | -100.0 °C | 1.82E-7 Ω·m Show Material materials with Resistividad eléctrica of 1.82E-7 Ω·m |
20.0 °C | 1.2E-7 - 2.47E-7 Ω·m Show Material materials with Resistividad eléctrica of 1.2E-7 - 2.47E-7 Ω·m | |
100.0 °C | 2.96E-7 Ω·m Show Material materials with Resistividad eléctrica of 2.96E-7 Ω·m | |
200.0 °C | 3.68E-7 Ω·m Show Material materials with Resistividad eléctrica of 3.68E-7 Ω·m | |
300.0 °C | 4.55E-7 Ω·m Show Material materials with Resistividad eléctrica of 4.55E-7 Ω·m | |
400.0 °C | 5.56E-7 Ω·m Show Material materials with Resistividad eléctrica of 5.56E-7 Ω·m | |
500.0 °C | 6.75E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.75E-7 Ω·m | |
600.0 °C | 8.13E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.13E-7 Ω·m | |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value |
---|---|
Azufre | 0.045 % Show Material materials with Azufre of 0.045 % |
Carbono | 0.17 - 0.24 % Show Material materials with Carbono of 0.17 - 0.24 % |
Fósforo | 0.05 % Show Material materials with Fósforo of 0.05 % |
Manganeso | 0.3 - 0.6 % Show Material materials with Manganeso of 0.3 - 0.6 % |
Silicona | 0.4 % Show Material materials with Silicona of 0.4 % |