General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.9 g/cm³ Show Material materials with Densidad of 7.9 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Austenitic Stainless Steel |
Elongación | -196.0 °C | 30 % Show Material materials with Elongación of 30 % | |
-150.0 °C | 30 % Show Material materials with Elongación of 30 % | ||
-80.0 °C | 35 % Show Material materials with Elongación of 35 % | ||
20.0 °C | 45 % Show Material materials with Elongación of 45 % | ||
Elongación A80 transversal | 20.0 °C | 45 % Show Material materials with Elongación A80 transversal of 45 % | |
Elongación transversal | 20.0 °C | 45 % Show Material materials with Elongación transversal of 45 % | |
Límite elástico Rp 0,2 | -196.0 °C | 300 MPa Show Material materials with Límite elástico Rp 0,2 of 300 MPa | |
-150.0 °C | 225 MPa Show Material materials with Límite elástico Rp 0,2 of 225 MPa | ||
-80.0 °C | 220 MPa Show Material materials with Límite elástico Rp 0,2 of 220 MPa | ||
20.0 °C | 200 MPa Show Material materials with Límite elástico Rp 0,2 of 200 MPa | ||
50.0 °C | 180 MPa Show Material materials with Límite elástico Rp 0,2 of 180 MPa | ||
100.0 °C | 147 MPa Show Material materials with Límite elástico Rp 0,2 of 147 MPa | ||
150.0 °C | 132 MPa Show Material materials with Límite elástico Rp 0,2 of 132 MPa | ||
200.0 °C | 118 MPa Show Material materials with Límite elástico Rp 0,2 of 118 MPa | ||
250.0 °C | 108 MPa Show Material materials with Límite elástico Rp 0,2 of 108 MPa | ||
300.0 °C | 100 MPa Show Material materials with Límite elástico Rp 0,2 of 100 MPa | ||
350.0 °C | 94 MPa Show Material materials with Límite elástico Rp 0,2 of 94 MPa | ||
400.0 °C | 89 MPa Show Material materials with Límite elástico Rp 0,2 of 89 MPa | ||
450.0 °C | 85 MPa Show Material materials with Límite elástico Rp 0,2 of 85 MPa | ||
500.0 °C | 81 MPa Show Material materials with Límite elástico Rp 0,2 of 81 MPa | ||
550.0 °C | 80 MPa Show Material materials with Límite elástico Rp 0,2 of 80 MPa | ||
Límite elástico Rp 1,0 | -196.0 °C | 400 MPa Show Material materials with Límite elástico Rp 1,0 of 400 MPa | |
-150.0 °C | 325 MPa Show Material materials with Límite elástico Rp 1,0 of 325 MPa | ||
-80.0 °C | 290 MPa Show Material materials with Límite elástico Rp 1,0 of 290 MPa | ||
20.0 °C | 240 MPa Show Material materials with Límite elástico Rp 1,0 of 240 MPa | ||
50.0 °C | 218 MPa Show Material materials with Límite elástico Rp 1,0 of 218 MPa | ||
100.0 °C | 181 MPa Show Material materials with Límite elástico Rp 1,0 of 181 MPa | ||
150.0 °C | 162 MPa Show Material materials with Límite elástico Rp 1,0 of 162 MPa | ||
200.0 °C | 147 MPa Show Material materials with Límite elástico Rp 1,0 of 147 MPa | ||
250.0 °C | 137 MPa Show Material materials with Límite elástico Rp 1,0 of 137 MPa | ||
300.0 °C | 127 MPa Show Material materials with Límite elástico Rp 1,0 of 127 MPa | ||
350.0 °C | 121 MPa Show Material materials with Límite elástico Rp 1,0 of 121 MPa | ||
400.0 °C | 116 MPa Show Material materials with Límite elástico Rp 1,0 of 116 MPa | ||
450.0 °C | 112 MPa Show Material materials with Límite elástico Rp 1,0 of 112 MPa | ||
500.0 °C | 109 MPa Show Material materials with Límite elástico Rp 1,0 of 109 MPa | ||
550.0 °C | 108 MPa Show Material materials with Límite elástico Rp 1,0 of 108 MPa | ||
Límite elástico transversal Rp 0,2 | 20.0 °C | 200 - 220 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 200 - 220 MPa | |
Límite elástico transversal Rp 1,0 | 20.0 °C | 240 - 250 MPa Show Material materials with Límite elástico transversal Rp 1,0 of 240 - 250 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Austenitic Stainless Steel |
Módulo elástico | 20.0 °C | 200 GPa Show Material materials with Módulo elástico of 200 GPa | |
100.0 °C | 194 GPa Show Material materials with Módulo elástico of 194 GPa | ||
200.0 °C | 186 GPa Show Material materials with Módulo elástico of 186 GPa | ||
300.0 °C | 179 GPa Show Material materials with Módulo elástico of 179 GPa | ||
400.0 °C | 172 GPa Show Material materials with Módulo elástico of 172 GPa | ||
500.0 °C | 165 GPa Show Material materials with Módulo elástico of 165 GPa | ||
Resistencia a la tracción | -196.0 °C | 1200 MPa Show Material materials with Resistencia a la tracción of 1200 MPa | |
-150.0 °C | 1070 MPa Show Material materials with Resistencia a la tracción of 1070 MPa | ||
-80.0 °C | 830 MPa Show Material materials with Resistencia a la tracción of 830 MPa | ||
20.0 °C | 500 - 700 MPa Show Material materials with Resistencia a la tracción of 500 - 700 MPa | ||
50.0 °C | 466 MPa Show Material materials with Resistencia a la tracción of 466 MPa | ||
100.0 °C | 410 MPa Show Material materials with Resistencia a la tracción of 410 MPa | ||
150.0 °C | 380 MPa Show Material materials with Resistencia a la tracción of 380 MPa | ||
200.0 °C | 360 MPa Show Material materials with Resistencia a la tracción of 360 MPa | ||
250.0 °C | 350 MPa Show Material materials with Resistencia a la tracción of 350 MPa | ||
300.0 °C | 340 MPa Show Material materials with Resistencia a la tracción of 340 MPa | ||
350.0 °C | 340 MPa Show Material materials with Resistencia a la tracción of 340 MPa | ||
Resistencia a la tracción transversal | 20.0 °C | 500 - 700 MPa Show Material materials with Resistencia a la tracción transversal of 500 - 700 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 500 J/(kg·K) Show Material materials with Calor específico of 500 J/(kg·K) | |
Coeficiente de dilatación térmica | 100.0 °C | 1.6E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 1/K | |
200.0 °C | 1.65E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.65E-5 1/K | ||
300.0 °C | 1.7E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.7E-5 1/K | ||
400.0 °C | 1.8E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 1/K | ||
500.0 °C | 1.8E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.8E-5 1/K | ||
Conductividad térmica | 20.0 °C | 15 W/(m·K) Show Material materials with Conductividad térmica of 15 W/(m·K) | |
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 7.3E-7 Ω·m Show Material materials with Resistividad eléctrica of 7.3E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.03 % Show Material materials with Carbono of 0.03 % |
Cromo | 17.5 - 19.5 % Show Material materials with Cromo of 17.5 - 19.5 % |
Fósforo | 0.05 % Show Material materials with Fósforo of 0.05 % |
Manganeso | 2 % Show Material materials with Manganeso of 2 % |
Nitrógeno | 0.1 - 0.11 % Show Material materials with Nitrógeno of 0.1 - 0.11 % |
Níquel | 8 - 10.5 % Show Material materials with Níquel of 8 - 10.5 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |