General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.65 - 7.7 g/cm³ Show Material materials with Densidad of 7.65 - 7.7 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Martensitic Stainless Steel |
Elongación | 20.0 °C | 12 - 14 % Show Material materials with Elongación of 12 - 14 % | |
Elongación transversal | 20.0 °C | 5 % Show Material materials with Elongación transversal of 5 % | |
Límite elástico | 20.0 °C | 550 MPa Show Material materials with Límite elástico of 550 MPa | |
Límite elástico Rp 0,2 | 20.0 °C | 550 MPa Show Material materials with Límite elástico Rp 0,2 of 550 MPa | |
50.0 °C | 515 MPa Show Material materials with Límite elástico Rp 0,2 of 515 MPa | ||
100.0 °C | 495 MPa Show Material materials with Límite elástico Rp 0,2 of 495 MPa | ||
150.0 °C | 475 MPa Show Material materials with Límite elástico Rp 0,2 of 475 MPa | ||
200.0 °C | 460 MPa Show Material materials with Límite elástico Rp 0,2 of 460 MPa | ||
250.0 °C | 450 MPa Show Material materials with Límite elástico Rp 0,2 of 450 MPa | ||
300.0 °C | 430 MPa Show Material materials with Límite elástico Rp 0,2 of 430 MPa | ||
350.0 °C | 390 MPa Show Material materials with Límite elástico Rp 0,2 of 390 MPa | ||
400.0 °C | 345 MPa Show Material materials with Límite elástico Rp 0,2 of 345 MPa | ||
Límite elástico transversal | 20.0 °C | 550 MPa Show Material materials with Límite elástico transversal of 550 MPa | |
Límite elástico transversal Rp 0,2 | 20.0 °C | 550 MPa Show Material materials with Límite elástico transversal Rp 0,2 of 550 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Martensitic Stainless Steel |
Módulo elástico | 20.0 °C | 196 - 216 GPa Show Material materials with Módulo elástico of 196 - 216 GPa | |
100.0 °C | 213 GPa Show Material materials with Módulo elástico of 213 GPa | ||
200.0 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | ||
300.0 °C | 200 GPa Show Material materials with Módulo elástico of 200 GPa | ||
400.0 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | ||
Resistencia a la tracción | 20.0 °C | 750 - 950 MPa Show Material materials with Resistencia a la tracción of 750 - 950 MPa | |
Resistencia a la tracción transversal | 20.0 °C | 750 - 950 MPa Show Material materials with Resistencia a la tracción transversal of 750 - 950 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 450 - 460 J/(kg·K) Show Material materials with Calor específico of 450 - 460 J/(kg·K) | |
100.0 °C | 482 J/(kg·K) Show Material materials with Calor específico of 482 J/(kg·K) | ||
200.0 °C | 506 J/(kg·K) Show Material materials with Calor específico of 506 J/(kg·K) | ||
300.0 °C | 525 J/(kg·K) Show Material materials with Calor específico of 525 J/(kg·K) | ||
400.0 °C | 547 J/(kg·K) Show Material materials with Calor específico of 547 J/(kg·K) | ||
500.0 °C | 576 J/(kg·K) Show Material materials with Calor específico of 576 J/(kg·K) | ||
600.0 °C | 616 J/(kg·K) Show Material materials with Calor específico of 616 J/(kg·K) | ||
Coeficiente de dilatación térmica | -100.0 °C | 9.2E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 9.2E-6 1/K | |
20.0 °C | 9.9E-6 1/K Show Material materials with Coeficiente de dilatación térmica of 9.9E-6 1/K | ||
100.0 °C | 1E-5 - 1.03E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1E-5 - 1.03E-5 1/K | ||
200.0 °C | 1.05E-5 - 1.08E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 - 1.08E-5 1/K | ||
300.0 °C | 1.1E-5 - 1.12E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.1E-5 - 1.12E-5 1/K | ||
400.0 °C | 1.1E-5 - 1.16E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.1E-5 - 1.16E-5 1/K | ||
500.0 °C | 1.1E-5 - 1.19E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.1E-5 - 1.19E-5 1/K | ||
600.0 °C | 1.21E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 1/K | ||
700.0 °C | 1.24E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.24E-5 1/K | ||
800.0 °C | 1.29E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.29E-5 1/K | ||
900.0 °C | 1.34E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.34E-5 1/K | ||
1000.0 °C | 1.39E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.39E-5 1/K | ||
Conductividad térmica | 20.0 °C | 19.6 - 25 W/(m·K) Show Material materials with Conductividad térmica of 19.6 - 25 W/(m·K) | |
Difusividad térmica | 20.0 °C | 5.7 mm²/s Show Material materials with Difusividad térmica of 5.7 mm²/s | |
Temperatura de fusión | 1370 - 1530 °C Show Material materials with Temperatura de fusión of 1370 - 1530 °C | Typical for Martensitic Stainless Steel |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 6.17E-7 - 7E-7 Ω·m Show Material materials with Resistividad eléctrica of 6.17E-7 - 7E-7 Ω·m |
Chemical properties
Property | Value |
---|---|
Azufre | 0.015 % Show Material materials with Azufre of 0.015 % |
Carbono | 0.12 - 0.22 % Show Material materials with Carbono of 0.12 - 0.22 % |
Cromo | 15 - 17 % Show Material materials with Cromo of 15 - 17 % |
Fósforo | 0.04 % Show Material materials with Fósforo of 0.04 % |
Manganeso | 1.5 % Show Material materials with Manganeso of 1.5 % |
Níquel | 1.5 - 2.5 % Show Material materials with Níquel of 1.5 - 2.5 % |
Silicona | 1 % Show Material materials with Silicona of 1 % |