DIN 17440 Grade X14CrMoS17 soft annealed (+A)

View suppliers (7)
Want to keep this datasheet? Save it now in your required format

Description

The material X14CrMoS17 is used acc. DIN 17440 : 1996-09 for rods (for pressure vessels), forgings and drawn wire. For the application acc. DIN 17440 : 1985-07 (X 12 CrMoS 17) resp. acc. DIN EN 10088-1,-2,-3 : 1995-08 (X14CrMoS17) applies: stainless free-cutting steel used in the quenched and tempered condition for construction parts like screws, nuts, fittings, axles, bolts, spindles in water, steam and weak alkaline and neutral media as well as for solenoid valves. Because of the S-content the corrosion resistance is comparable to an steel with 13% Cr.

Related Standards

Equivalent Materials

Los datos sobre este material han sido proporcionados por WIAM.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValue

Densidad

20.0 °C

7.65 - 7.7 g/cm³

Show Material materials with Densidad of 7.65 - 7.7 g/cm³

Mecánica

PropertyTemperatureValueComment

Coeficiente de Poisson

23.0 °C

0.3 [-]

Show Material materials with Coeficiente de Poisson of 0.3 [-]

Typical for Ferritic Stainless Steel

Dureza Brinell

20.0 °C

230 [-]

Show Material materials with Dureza Brinell of 230 [-]

Dureza Vickers

20.0 °C

230 [-]

Show Material materials with Dureza Vickers of 230 [-]

Elongación

20.0 °C

16 %

Show Material materials with Elongación of 16 %

Módulo de cizallamiento

23.0 °C

77 GPa

Show Material materials with Módulo de cizallamiento of 77 GPa

Typical for Ferritic Stainless Steel

Módulo elástico

20.0 °C

196 - 216 GPa

Show Material materials with Módulo elástico of 196 - 216 GPa

100.0 °C

213 GPa

Show Material materials with Módulo elástico of 213 GPa

200.0 °C

207 GPa

Show Material materials with Módulo elástico of 207 GPa

300.0 °C

200 GPa

Show Material materials with Módulo elástico of 200 GPa

400.0 °C

192 GPa

Show Material materials with Módulo elástico of 192 GPa

Resistencia a la tracción

20.0 °C

540 - 740 MPa

Show Material materials with Resistencia a la tracción of 540 - 740 MPa

Aplicaciones térmicas

PropertyTemperatureValueComment

Calor específico

20.0 °C

450 - 460 J/(kg·K)

Show Material materials with Calor específico of 450 - 460 J/(kg·K)

100.0 °C

482 J/(kg·K)

Show Material materials with Calor específico of 482 J/(kg·K)

200.0 °C

506 J/(kg·K)

Show Material materials with Calor específico of 506 J/(kg·K)

300.0 °C

525 J/(kg·K)

Show Material materials with Calor específico of 525 J/(kg·K)

400.0 °C

547 J/(kg·K)

Show Material materials with Calor específico of 547 J/(kg·K)

500.0 °C

576 J/(kg·K)

Show Material materials with Calor específico of 576 J/(kg·K)

600.0 °C

616 J/(kg·K)

Show Material materials with Calor específico of 616 J/(kg·K)

Unlock all property charts

Coeficiente de dilatación térmica

-100.0 °C

9.2E-6 1/K

Show Material materials with Coeficiente de dilatación térmica of 9.2E-6 1/K

20.0 °C

9.9E-6 1/K

Show Material materials with Coeficiente de dilatación térmica of 9.9E-6 1/K

100.0 °C

1E-5 - 1.03E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1E-5 - 1.03E-5 1/K

200.0 °C

1.05E-5 - 1.08E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 - 1.08E-5 1/K

300.0 °C

1.05E-5 - 1.12E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 - 1.12E-5 1/K

400.0 °C

1.05E-5 - 1.16E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.05E-5 - 1.16E-5 1/K

500.0 °C

1.1E-5 - 1.19E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.1E-5 - 1.19E-5 1/K

600.0 °C

1.21E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 1/K

700.0 °C

1.24E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.24E-5 1/K

800.0 °C

1.29E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.29E-5 1/K

900.0 °C

1.34E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.34E-5 1/K

1000.0 °C

1.39E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.39E-5 1/K

Unlock all property charts

Conductividad térmica

20.0 °C

19.6 - 25 W/(m·K)

Show Material materials with Conductividad térmica of 19.6 - 25 W/(m·K)

Difusividad térmica

20.0 °C

5.7 mm²/s

Show Material materials with Difusividad térmica of 5.7 mm²/s

Temperatura de fusión

1425 - 1530 °C

Show Material materials with Temperatura de fusión of 1425 - 1530 °C

Typical for Ferritic Stainless Steel

Eléctrico

PropertyTemperatureValue

Resistividad eléctrica

20.0 °C

6.17E-7 - 7E-7 Ω·m

Show Material materials with Resistividad eléctrica of 6.17E-7 - 7E-7 Ω·m

Chemical properties

PropertyValue

Azufre

0.15 - 0.35 %

Show Material materials with Azufre of 0.15 - 0.35 %

Carbono

0.1 - 0.17 %

Show Material materials with Carbono of 0.1 - 0.17 %

Cromo

15.5 - 17.5 %

Show Material materials with Cromo of 15.5 - 17.5 %

Fósforo

0.04 %

Show Material materials with Fósforo of 0.04 %

Manganeso

1.5 %

Show Material materials with Manganeso of 1.5 %

Molibdeno

0.2 - 0.6 %

Show Material materials with Molibdeno of 0.2 - 0.6 %

Silicona

1 %

Show Material materials with Silicona of 1 %