General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 7.83 g/cm³ Show Material materials with Densidad of 7.83 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.29 [-] Show Material materials with Coeficiente de Poisson of 0.29 [-] | Typical for Chromium Molybdenum Steel |
Dureza Rockwell B | 23.0 °C | 90 [-] Show Material materials with Dureza Rockwell B of 90 [-] | Annealed |
Dureza Vickers | 23.0 °C | 340 - 490 [-] Show Material materials with Dureza Vickers of 340 - 490 [-] | Quenched and Tempered - Annealed: Max=195 |
Elongación | 23.0 °C | 15 % Show Material materials with Elongación of 15 % | Annealed |
Límite elástico Rp 0,2 | 23.0 °C | 480 MPa Show Material materials with Límite elástico Rp 0,2 of 480 MPa | Annealed |
Módulo elástico | 23.0 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | |
Resistencia a la tracción | 23.0 °C | 1100 - 1600 MPa Show Material materials with Resistencia a la tracción of 1100 - 1600 MPa | Quenched and Tempered condition - Annealed condition: Max=620 |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 448 - 502 J/(kg·K) Show Material materials with Calor específico of 448 - 502 J/(kg·K) | Typical for Chromium Molybdenum Steel |
Coeficiente de dilatación térmica | 20.0 °C | 1.15E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.15E-5 1/K | |
100.0 °C | 1.21E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.21E-5 1/K | ||
200.0 °C | 1.27E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.27E-5 1/K | ||
300.0 °C | 1.32E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.32E-5 1/K | ||
400.0 °C | 1.36E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36E-5 1/K | ||
Conductividad térmica | 20.0 °C | 45.1 W/(m·K) Show Material materials with Conductividad térmica of 45.1 W/(m·K) | |
200.0 °C | 44.1 W/(m·K) Show Material materials with Conductividad térmica of 44.1 W/(m·K) | ||
300.0 °C | 41.9 W/(m·K) Show Material materials with Conductividad térmica of 41.9 W/(m·K) | ||
400.0 °C | 39.4 W/(m·K) Show Material materials with Conductividad térmica of 39.4 W/(m·K) | ||
500.0 °C | 36.9 W/(m·K) Show Material materials with Conductividad térmica of 36.9 W/(m·K) | ||
Temperatura de fusión | 1382 - 1529 °C Show Material materials with Temperatura de fusión of 1382 - 1529 °C | Typical for Chromium Molybdenum Steel |
Chemical properties
Property | Value |
---|---|
Carbono | 0.38 - 0.45 % Show Material materials with Carbono of 0.38 - 0.45 % |
Cromo | 0.9 - 1.2 % Show Material materials with Cromo of 0.9 - 1.2 % |
Manganeso | 0.5 - 0.8 % Show Material materials with Manganeso of 0.5 - 0.8 % |
Molibdeno | 0.15 - 0.25 % Show Material materials with Molibdeno of 0.15 - 0.25 % |
Silicona | 0.17 - 0.37 % Show Material materials with Silicona of 0.17 - 0.37 % |