The make X3CrNiMoN27-5-2 is comparable to X 4 CrNiMoN 27 5 2 acc. to SEW400 : 1991. The ferritic-austensitic steel shows low stress corrosion sensitivity. It shows better general corrosion resistance than 1.4362 and better machinability than austenites. The steel is charactrized by high abrasion resistance and favorable running characteristics, it is usable for mirror finishing. Therefore particularly suitable for shafts in acid pumps and for seawater exposed machine components. Further application in acetic acid, photo, cellulose and in dyeing industry. The material shows resistance to intercrystalline corrosion also in welded condition.

Related Standards

Equivalent Materials

Los datos sobre este material han sido proporcionados por WIAM.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValue

Densidad

20.0 °C

7.8 - 7.82 g/cm³

Show Material materials with Densidad of 7.8 - 7.82 g/cm³

Mecánica

PropertyTemperatureValueComment

Coeficiente de Poisson

23.0 °C

0.3 [-]

Show Material materials with Coeficiente de Poisson of 0.3 [-]

Typical for Duplex Stainless Steel

Elongación

20.0 °C

20 %

Show Material materials with Elongación of 20 %

Elongación transversal

20.0 °C

15 %

Show Material materials with Elongación transversal of 15 %

Límite elástico Rp 0,2

20.0 °C

460 MPa

Show Material materials with Límite elástico Rp 0,2 of 460 MPa

100.0 °C

360 MPa

Show Material materials with Límite elástico Rp 0,2 of 360 MPa

150.0 °C

335 MPa

Show Material materials with Límite elástico Rp 0,2 of 335 MPa

200.0 °C

310 MPa

Show Material materials with Límite elástico Rp 0,2 of 310 MPa

250.0 °C

295 MPa

Show Material materials with Límite elástico Rp 0,2 of 295 MPa

Módulo de cizallamiento

23.0 °C

77 GPa

Show Material materials with Módulo de cizallamiento of 77 GPa

Typical for Duplex Stainless Steel

Módulo elástico

20.0 °C

200 - 212 GPa

Show Material materials with Módulo elástico of 200 - 212 GPa

100.0 °C

194 - 206 GPa

Show Material materials with Módulo elástico of 194 - 206 GPa

200.0 °C

186 GPa

Show Material materials with Módulo elástico of 186 GPa

300.0 °C

180 GPa

Show Material materials with Módulo elástico of 180 GPa

Unlock all property charts

Resistencia a la tracción

20.0 °C

620 - 880 MPa

Show Material materials with Resistencia a la tracción of 620 - 880 MPa

Resistencia a la tracción transversal

20.0 °C

620 - 880 MPa

Show Material materials with Resistencia a la tracción transversal of 620 - 880 MPa

Aplicaciones térmicas

PropertyTemperatureValueComment

Calor específico

20.0 °C

500 J/(kg·K)

Show Material materials with Calor específico of 500 J/(kg·K)

Coeficiente de dilatación térmica

100.0 °C

1.3E-5 - 1.33E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.3E-5 - 1.33E-5 1/K

200.0 °C

1.35E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.35E-5 1/K

300.0 °C

1.4E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.4E-5 1/K

Unlock all property charts

Conductividad térmica

20.0 °C

13.4 - 15 W/(m·K)

Show Material materials with Conductividad térmica of 13.4 - 15 W/(m·K)

100.0 °C

14.9 W/(m·K)

Show Material materials with Conductividad térmica of 14.9 W/(m·K)

Unlock all property charts

Temperatura de fusión

1375 - 1450 °C

Show Material materials with Temperatura de fusión of 1375 - 1450 °C

Typical for Duplex Stainless Steel

Temperatura máx. de funcionamiento

300 °C

Show Material materials with Temperatura máx. de funcionamiento of 300 °C

Typical for Duplex Stainless Steel

Eléctrico

PropertyTemperatureValue

Resistividad eléctrica

20.0 °C

7.85E-7 Ω·m

Show Material materials with Resistividad eléctrica of 7.85E-7 Ω·m

100.0 °C

8.44E-7 Ω·m

Show Material materials with Resistividad eléctrica of 8.44E-7 Ω·m

Unlock all property charts

Chemical properties

PropertyValue

Azufre

0.03 %

Show Material materials with Azufre of 0.03 %

Carbono

0.05 %

Show Material materials with Carbono of 0.05 %

Cromo

25 - 28 %

Show Material materials with Cromo of 25 - 28 %

Fósforo

0.04 %

Show Material materials with Fósforo of 0.04 %

Manganeso

2 %

Show Material materials with Manganeso of 2 %

Molibdeno

1.3 - 2 %

Show Material materials with Molibdeno of 1.3 - 2 %

Nitrógeno

0.05 - 0.2 %

Show Material materials with Nitrógeno of 0.05 - 0.2 %

Níquel

4.5 - 6.5 %

Show Material materials with Níquel of 4.5 - 6.5 %

Silicona

1 %