General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 20 °C | 7.85 g/cm³ Show Material materials with Densidad of 7.85 g/cm³ | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20 °C | 0.284 [-] Show Material materials with Coeficiente de Poisson of 0.284 [-] | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | |
Dureza Brinell | 247 [-] Show Material materials with Dureza Brinell of 247 [-] | Predicted Value, Transverse | ||||
Elongación | 18.0 % Show Material materials with Elongación of 18.0 % | Predicted Value, A200 | ||||
18.3 % Show Material materials with Elongación of 18.3 % | Predicted Value, A80 Transverse | |||||
19 % Show Material materials with Elongación of 19 % | Predicted Value, Transverse | |||||
22.1 % Show Material materials with Elongación of 22.1 % | Predicted Value, A5 | |||||
24.8 % Show Material materials with Elongación of 24.8 % | Predicted Value, A50 | |||||
25.2 % Show Material materials with Elongación of 25.2 % | Predicted Value | |||||
20 °C | 17 % Show Material materials with Elongación of 17 % | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | A80 | |
20 °C | 18 % Show Material materials with Elongación of 18 % | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | A80 | |
20 °C | 19 % Show Material materials with Elongación of 19 % | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | A80 | |
20 °C | 20 % Show Material materials with Elongación of 20 % | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | A80 | |
20 °C | 21 % Show Material materials with Elongación of 21 % | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | A80 | |
Estricción | 42.1 % Show Material materials with Estricción of 42.1 % | Predicted Value | ||||
43.4 % Show Material materials with Estricción of 43.4 % | Predicted Value, Transverse | |||||
Límite elástico | 260 MPa Show Material materials with Límite elástico of 260 MPa | Predicted Value, RP1 | ||||
292.7 MPa Show Material materials with Límite elástico of 292.7 MPa | Predicted Value, Transverse | |||||
294.7 MPa Show Material materials with Límite elástico of 294.7 MPa | Predicted Value, RP05 | |||||
318.2 MPa Show Material materials with Límite elástico of 318.2 MPa | Predicted Value, RP1 Transverse | |||||
336.3 MPa Show Material materials with Límite elástico of 336.3 MPa | Predicted Value, RP02 | |||||
469.3 MPa Show Material materials with Límite elástico of 469.3 MPa | Predicted Value, RP02 Transverse | |||||
477.1 MPa Show Material materials with Límite elástico of 477.1 MPa | Predicted Value, RP002 | |||||
20 °C | 225 MPa Show Material materials with Límite elástico of 225 MPa | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
20 °C | 235 MPa Show Material materials with Límite elástico of 235 MPa | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
Módulo de cizallamiento | 82 GPa Show Material materials with Módulo de cizallamiento of 82 GPa | Typical for Low Carbon Steel | ||||
Módulo elástico | -100 °C | 217 GPa Show Material materials with Módulo elástico of 217 GPa | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | |
20 °C | 212 GPa Show Material materials with Módulo elástico of 212 GPa | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
100 °C | 207 GPa Show Material materials with Módulo elástico of 207 GPa | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
200 °C | 199 GPa Show Material materials with Módulo elástico of 199 GPa | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
300 °C | 192 GPa Show Material materials with Módulo elástico of 192 GPa | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
400 °C | 184 GPa Show Material materials with Módulo elástico of 184 GPa | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
500 °C | 175 GPa Show Material materials with Módulo elástico of 175 GPa | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
600 °C | 164 GPa Show Material materials with Módulo elástico of 164 GPa | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
Resistencia a la tracción | 20 °C | 340 - 510 MPa Show Material materials with Resistencia a la tracción of 340 - 510 MPa | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | |
20 °C | 340 - 470 MPa Show Material materials with Resistencia a la tracción of 340 - 470 MPa | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
20 °C | 360 - 510 MPa Show Material materials with Resistencia a la tracción of 360 - 510 MPa | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
20 °C | 360 - 470 MPa Show Material materials with Resistencia a la tracción of 360 - 470 MPa | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
Resistencia al cizallamiento | 510 MPa Show Material materials with Resistencia al cizallamiento of 510 MPa | Predicted Value |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | -100 °C | 423 J/(kg·K) Show Material materials with Calor específico of 423 J/(kg·K) | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | |
20 °C | 461 J/(kg·K) Show Material materials with Calor específico of 461 J/(kg·K) | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
100 °C | 479 J/(kg·K) Show Material materials with Calor específico of 479 J/(kg·K) | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
200 °C | 499 J/(kg·K) Show Material materials with Calor específico of 499 J/(kg·K) | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
300 °C | 517 J/(kg·K) Show Material materials with Calor específico of 517 J/(kg·K) | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
400 °C | 536 J/(kg·K) Show Material materials with Calor específico of 536 J/(kg·K) | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
500 °C | 558 J/(kg·K) Show Material materials with Calor específico of 558 J/(kg·K) | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
600 °C | 587 J/(kg·K) Show Material materials with Calor específico of 587 J/(kg·K) | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
Coeficiente de dilatación térmica | -100 °C | 1.08e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.08e-05 1/K | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | |
20 °C | 1.19e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.19e-05 1/K | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
100 °C | 1.25e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.25e-05 1/K | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
200 °C | 1.3e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.3e-05 1/K | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
300 °C | 1.36e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.36e-05 1/K | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
400 °C | 1.41e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.41e-05 1/K | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
500 °C | 1.45e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.45e-05 1/K | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
600 °C | 1.49e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 1.49e-05 1/K | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
Conductividad térmica | 20 °C | 56.9 W/(m·K) Show Material materials with Conductividad térmica of 56.9 W/(m·K) | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | |
100 °C | 56.4 W/(m·K) Show Material materials with Conductividad térmica of 56.4 W/(m·K) | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
200 °C | 53.5 W/(m·K) Show Material materials with Conductividad térmica of 53.5 W/(m·K) | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
300 °C | 49.4 W/(m·K) Show Material materials with Conductividad térmica of 49.4 W/(m·K) | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
400 °C | 45.2 W/(m·K) Show Material materials with Conductividad térmica of 45.2 W/(m·K) | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
500 °C | 41.3 W/(m·K) Show Material materials with Conductividad térmica of 41.3 W/(m·K) | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
600 °C | 37.6 W/(m·K) Show Material materials with Conductividad térmica of 37.6 W/(m·K) | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
Difusividad térmica | 20 °C | 15.7 mm²/s Show Material materials with Difusividad térmica of 15.7 mm²/s | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | |
100 °C | 14.5 mm²/s Show Material materials with Difusividad térmica of 14.5 mm²/s | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
200 °C | 12.9 mm²/s Show Material materials with Difusividad térmica of 12.9 mm²/s | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
300 °C | 11.2 mm²/s Show Material materials with Difusividad térmica of 11.2 mm²/s | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
400 °C | 9.6 mm²/s Show Material materials with Difusividad térmica of 9.6 mm²/s | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
500 °C | 7.9 mm²/s Show Material materials with Difusividad térmica of 7.9 mm²/s | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
600 °C | 6.3 mm²/s Show Material materials with Difusividad térmica of 6.3 mm²/s | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
Temperatura de fusión | 1480 - 1526 °C Show Material materials with Temperatura de fusión of 1480 - 1526 °C | Typical for Low Carbon Steel | ||||
Temperatura máx. de funcionamiento | 391.1 °C Show Material materials with Temperatura máx. de funcionamiento of 391.1 °C | Predicted Value, Long | ||||
500 °C Show Material materials with Temperatura máx. de funcionamiento of 500 °C | Typical for Carbon Steel |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Conductividad eléctrica | 8 S/m Show Material materials with Conductividad eléctrica of 8 S/m | Predicted Value | ||||
Resistividad eléctrica | 20 °C | 1.83e-07 Ω·m Show Material materials with Resistividad eléctrica of 1.83e-07 Ω·m | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | |
100 °C | 2.27e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.27e-07 Ω·m | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
200 °C | 2.95e-07 Ω·m Show Material materials with Resistividad eléctrica of 2.95e-07 Ω·m | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
300 °C | 3.8e-07 Ω·m Show Material materials with Resistividad eléctrica of 3.8e-07 Ω·m | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
400 °C | 4.81e-07 Ω·m Show Material materials with Resistividad eléctrica of 4.81e-07 Ω·m | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
500 °C | 5.99e-07 Ω·m Show Material materials with Resistividad eléctrica of 5.99e-07 Ω·m | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat | ||
600 °C | 7.38e-07 Ω·m Show Material materials with Resistividad eléctrica of 7.38e-07 Ω·m | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat |
Magnético
Property | Value | Comment |
---|---|---|
Temperatura de Curie | 770 °C Show Material materials with Temperatura de Curie of 770 °C | Typical for Low Carbon Steel |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Azufre | 0.045 % Show Material materials with Azufre of 0.045 % | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat |
Carbono | 0.17 % Show Material materials with Carbono of 0.17 % | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat |
Fósforo | 0.045 % Show Material materials with Fósforo of 0.045 % | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat |
Manganeso | 1.4 % Show Material materials with Manganeso of 1.4 % | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat |
Nitrógeno | 0.009 % Show Material materials with Nitrógeno of 0.009 % | as-rolled condition (+AR) | EN 10025, EN 10025-1, EN 10025-2 | Sheet, Strip, Flat |