EN 1652 Grade Cu-DLP R200

View suppliers (9)
Want to keep this datasheet? Save it now in your required format

Description

Cu-DLP, mat. No CW023A, is a deoxidized copper with limited, low residual copper-content. To the comparable DIN-make SW-Cu, mat. No 2.0076 acc. to DIN 1787 : 1973-01 applies: Tensile strength and Brinell hardness are increasable by cold forming. SW-Cu is hydrogen resistant and shows the lowest thermal and electrical conductivity of the pure copper materials. Processing properties: hot forming: very good cold forming: very good machinability: unfavorable hard soldering: very good soft soldering: very good gas-shielded welding: good burnishing: very good Application: Preferably in apparatus engineering and construction trade. For the electrolytically tinned strip the coatings (Sn bright, Sn matt, Sn fuzed, SnPb) are listed by the application (better solderability, better corrosion resistance, reduction of the electrical contact resistance, better appearance) in the DIN EN 14436 : 2004-11 (Table 5)

Related Standards

Equivalent Materials

Los datos sobre este material han sido proporcionados por WIAM.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Propiedades

General

PropertyTemperatureValue

Densidad

20.0 °C

8.9 - 8.94 g/cm³

Show Material materials with Densidad of 8.9 - 8.94 g/cm³

Mecánica

PropertyTemperatureValueComment

Coeficiente de Poisson

20.0 °C

0.34 [-]

Show Material materials with Coeficiente de Poisson of 0.34 [-]

Dureza Vickers

20.0 °C

55 [-]

Show Material materials with Dureza Vickers of 55 [-]

Elongación

20.0 °C

33 - 42 %

Show Material materials with Elongación of 33 - 42 %

Límite elástico Rp 0,2

20.0 °C

40 - 100 MPa

Show Material materials with Límite elástico Rp 0,2 of 40 - 100 MPa

Límite elástico Rp 1,0

50.0 °C

60 MPa

Show Material materials with Límite elástico Rp 1,0 of 60 MPa

100.0 °C

55 MPa

Show Material materials with Límite elástico Rp 1,0 of 55 MPa

150.0 °C

55 MPa

Show Material materials with Límite elástico Rp 1,0 of 55 MPa

Módulo de cizallamiento

23.0 °C

48 GPa

Show Material materials with Módulo de cizallamiento of 48 GPa

Typical for Wrought Copper Pure / Low Alloyed Copper

Módulo elástico

20.0 °C

129 - 132 GPa

Show Material materials with Módulo elástico of 129 - 132 GPa

Resistencia a la tracción

20.0 °C

200 - 250 MPa

Show Material materials with Resistencia a la tracción of 200 - 250 MPa

Aplicaciones térmicas

PropertyTemperatureValueComment

Calor específico

20.0 °C

385 - 386 J/(kg·K)

Show Material materials with Calor específico of 385 - 386 J/(kg·K)

Coeficiente de dilatación térmica

23.0 °C

1.6E-5 - 1.8E-5 1/K

Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 - 1.8E-5 1/K

Typical for Wrought Copper Pure / Low Alloyed Copper

Conductividad térmica

20.0 °C

350 - 352 W/(m·K)

Show Material materials with Conductividad térmica of 350 - 352 W/(m·K)

Temperatura de fusión

965 - 1100 °C

Show Material materials with Temperatura de fusión of 965 - 1100 °C

Typical for Wrought Copper Pure / Low Alloyed Copper

Eléctrico

PropertyTemperatureValue

Conductividad eléctrica

20.0 °C

5.20E+7 S/m

Show Material materials with Conductividad eléctrica of 5.20E+7 S/m

Resistividad eléctrica

20.0 °C

1.9E-8 Ω·m

Show Material materials with Resistividad eléctrica of 1.9E-8 Ω·m

Chemical properties

PropertyValue

Bismuto

5E-4 %

Show Material materials with Bismuto of 5E-4 %

Cobre

99.9 %

Show Material materials with Cobre of 99.9 %

Fósforo

0.01 %

Show Material materials with Fósforo of 0.01 %

Plomo

5E-3 %

Show Material materials with Plomo of 5E-3 %