General
Property | Temperature | Value |
---|---|---|
Densidad | 20.0 °C | 7.6 g/cm³ Show Material materials with Densidad of 7.6 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | Typical for Leaded Phosphor Bronze |
Dureza Brinell | 20.0 °C | 140 - 180 [-] Show Material materials with Dureza Brinell of 140 - 180 [-] | |
Dureza Vickers | 20.0 °C | 145 - 185 [-] Show Material materials with Dureza Vickers of 145 - 185 [-] | |
Módulo de cizallamiento | 20.0 °C | 43 GPa Show Material materials with Módulo de cizallamiento of 43 GPa | |
Módulo elástico | 20.0 °C | 120 GPa Show Material materials with Módulo elástico of 120 GPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 20.0 °C | 377 - 418 J/(kg·K) Show Material materials with Calor específico of 377 - 418 J/(kg·K) | |
Coeficiente de dilatación térmica | 23.0 °C | 1.5E-5 - 1.9E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.5E-5 - 1.9E-5 1/K | Typical for Leaded Phosphor Bronze |
Conductividad térmica | 20.0 °C | 57 W/(m·K) Show Material materials with Conductividad térmica of 57 W/(m·K) |
Eléctrico
Property | Temperature | Value |
---|---|---|
Conductividad eléctrica | 20.0 °C | 7.00E+6 S/m Show Material materials with Conductividad eléctrica of 7.00E+6 S/m |
Specific Electrical conductivity | 12.1 % IACS Show Material materials with Specific Electrical conductivity of 12.1 % IACS |
Chemical properties
Property | Value |
---|---|
Aluminio | 9 - 11 % Show Material materials with Aluminio of 9 - 11 % |
Cobre | 79.45 % Show Material materials with Cobre of 79.45 % |
Estaño | 0.1 % Show Material materials with Estaño of 0.1 % |
Hierro | 2 - 4 % Show Material materials with Hierro of 2 - 4 % |
Manganeso | 1.5 - 3.5 % Show Material materials with Manganeso of 1.5 - 3.5 % |
Níquel | 1 % Show Material materials with Níquel of 1 % |
Plomo | 0.05 % Show Material materials with Plomo of 0.05 % |
Silicona | 0.2 % Show Material materials with Silicona of 0.2 % |
Zinc | 0.5 % Show Material materials with Zinc of 0.5 % |