General
Property | Value | Condition |
---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | F |
Mecánica
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | F | |||
Dureza Brinell | 55.0 [-] Show Material materials with Dureza Brinell of 55.0 [-] | F | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
Elongación | 2.0 % Show Material materials with Elongación of 2.0 % | F | Pink Sheets, ASTM B26, ASTM B618 | Casting | A100 |
3.0 % Show Material materials with Elongación of 3.0 % | F | Pink Sheets, ASTM B108 | Casting | A100 | |
3.8 % Show Material materials with Elongación of 3.8 % | F | ||||
6 % Show Material materials with Elongación of 6 % | F | Sand cast, elongation in 50 mm | |||
Límite elástico | 65.0 MPa Show Material materials with Límite elástico of 65.0 MPa | F | Pink Sheets, ASTM B26 | Casting | RP02 |
70.0 MPa Show Material materials with Límite elástico of 70.0 MPa | F | Pink Sheets, ASTM B108 | Casting | RP02 | |
100.0 MPa Show Material materials with Límite elástico of 100.0 MPa | F | ||||
124 MPa Show Material materials with Límite elástico of 124 MPa | F | Sand cast, RP02 | |||
Módulo de cizallamiento | 27.2 GPa Show Material materials with Módulo de cizallamiento of 27.2 GPa | F | |||
Módulo elástico | 72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | F | |||
72.4 GPa Show Material materials with Módulo elástico of 72.4 GPa | F | ||||
Resistencia a la tracción | 130.0 MPa Show Material materials with Resistencia a la tracción of 130.0 MPa | F | Pink Sheets, ASTM B26, ASTM B618 | Casting | |
145.0 MPa Show Material materials with Resistencia a la tracción of 145.0 MPa | F | Pink Sheets, ASTM B108 | Casting | ||
164 MPa Show Material materials with Resistencia a la tracción of 164 MPa | F | Sand cast |
Aplicaciones térmicas
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Calor específico | 970.0 J/(kg·K) Show Material materials with Calor específico of 970.0 J/(kg·K) | F | ||
Coeficiente de dilatación térmica | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | F | ||
Conductividad térmica | 160.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 W/(m·K) | F | ||
Temperatura de fusión | 557.0 - 613.0 °C Show Material materials with Temperatura de fusión of 557.0 - 613.0 °C | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
570.0 °C Show Material materials with Temperatura de fusión of 570.0 °C | F |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 90.1 - 93.3 % Show Material materials with Aluminio of 90.1 - 93.3 % | F | ||
Cobre | 0.25 % Show Material materials with Cobre of 0.25 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Hierro | 0.6 % Show Material materials with Hierro of 0.6 % | F | ||
0.60 % Show Material materials with Hierro of 0.60 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting | |
Magnesio | 0.2 - 0.45 % Show Material materials with Magnesio of 0.2 - 0.45 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Manganeso | 0.35 % Show Material materials with Manganeso of 0.35 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | F | ||
Silicona | 6.5 - 7.5 % Show Material materials with Silicona of 6.5 - 7.5 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Titanio | 0.25 % Show Material materials with Titanio of 0.25 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |
Zinc | 0.35 % Show Material materials with Zinc of 0.35 % | F | Pink Sheets, ASTM B108, ASTM B26, ASTM B618 | Casting |