General
Property | Value | Condition |
---|---|---|
Densidad | 2.7 g/cm³ Show Material materials with Densidad of 2.7 g/cm³ | T6 |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | T6 | ||||
Compressive yield strength | 172.0 - 186.0 MPa Show Material materials with Compressive yield strength of 172.0 - 186.0 MPa | T6 | ||||
Dureza Brinell | 70.0 [-] Show Material materials with Dureza Brinell of 70.0 [-] | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | ||
80 [-] Show Material materials with Dureza Brinell of 80 [-] | T6 | 500 kg load, 10 mm b | ||||
85.0 [-] Show Material materials with Dureza Brinell of 85.0 [-] | T6 | Pink Sheets, ASTM B108, ASTM B955 | Casting | |||
Elongación | -195 °C | 3.5 % Show Material materials with Elongación of 3.5 % | T6 | Sand cast, elongation in 50 mm | ||
-80 °C | 3.5 % Show Material materials with Elongación of 3.5 % | T6 | Sand cast, elongation in 50 mm | |||
-28 °C | 3.5 % Show Material materials with Elongación of 3.5 % | T6 | Sand cast, elongation in 50 mm | |||
3.0 % Show Material materials with Elongación of 3.0 % | T6 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955 | Casting | A100 | ||
3.8 % Show Material materials with Elongación of 3.8 % | T6 | |||||
24 °C | 3.5 % Show Material materials with Elongación of 3.5 % | T6 | Sand cast, elongation in 50 mm | |||
100 °C | 4 % Show Material materials with Elongación of 4 % | T6 | Sand cast, elongation in 50 mm | |||
150 °C | 6 % Show Material materials with Elongación of 6 % | T6 | Sand cast, elongation in 50 mm | |||
205 °C | 18 % Show Material materials with Elongación of 18 % | T6 | Sand cast, elongation in 50 mm | |||
260 °C | 35 % Show Material materials with Elongación of 35 % | T6 | Sand cast, elongation in 50 mm | |||
315 °C | 60 % Show Material materials with Elongación of 60 % | T6 | Sand cast, elongation in 50 mm | |||
371 °C | 80 % Show Material materials with Elongación of 80 % | T6 | Sand cast, elongation in 50 mm | |||
Límite elástico | -195 °C | 193 MPa Show Material materials with Límite elástico of 193 MPa | T6 | Sand cast, RP02 | ||
-80 °C | 172 MPa Show Material materials with Límite elástico of 172 MPa | T6 | Sand cast, RP02 | |||
-28 °C | 165 MPa Show Material materials with Límite elástico of 165 MPa | T6 | Sand cast, RP02 | |||
140.0 MPa Show Material materials with Límite elástico of 140.0 MPa | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | RP02 | ||
150.0 MPa Show Material materials with Límite elástico of 150.0 MPa | T6 | Pink Sheets, ASTM B108, ASTM B955 | Casting | RP02 | ||
170.0 MPa Show Material materials with Límite elástico of 170.0 MPa | T6 | |||||
24 °C | 165 MPa Show Material materials with Límite elástico of 165 MPa | T6 | Sand cast, RP02 | |||
100 °C | 165 MPa Show Material materials with Límite elástico of 165 MPa | T6 | Sand cast, RP02 | |||
150 °C | 138 MPa Show Material materials with Límite elástico of 138 MPa | T6 | Sand cast, RP02 | |||
205 °C | 58 MPa Show Material materials with Límite elástico of 58 MPa | T6 | Sand cast, RP02 | |||
260 °C | 35 MPa Show Material materials with Límite elástico of 35 MPa | T6 | Sand cast, RP02 | |||
315 °C | 21 MPa Show Material materials with Límite elástico of 21 MPa | T6 | Sand cast, RP02 | |||
371 °C | 14 MPa Show Material materials with Límite elástico of 14 MPa | T6 | Sand cast, RP02 | |||
Módulo de cizallamiento | 27.2 GPa Show Material materials with Módulo de cizallamiento of 27.2 GPa | T6 | ||||
Módulo elástico | 72.0 GPa Show Material materials with Módulo elástico of 72.0 GPa | T6 | ||||
72.4 GPa Show Material materials with Módulo elástico of 72.4 GPa | T6 | |||||
Resistencia a la fatiga | 90 MPa Show Material materials with Resistencia a la fatiga of 90 MPa | T6 | for 5x10⁸ cycles, R.R. Moore type test | |||
Resistencia a la tracción | -195 °C | 275 MPa Show Material materials with Resistencia a la tracción of 275 MPa | T6 | Sand cast | ||
-80 °C | 240 MPa Show Material materials with Resistencia a la tracción of 240 MPa | T6 | Sand cast | |||
-28 °C | 227 MPa Show Material materials with Resistencia a la tracción of 227 MPa | T6 | Sand cast | |||
205.0 MPa Show Material materials with Resistencia a la tracción of 205.0 MPa | T6 | Pink Sheets, ASTM B26, ASTM B618 | Casting | |||
220.0 MPa Show Material materials with Resistencia a la tracción of 220.0 MPa | T6 | |||||
230.0 MPa Show Material materials with Resistencia a la tracción of 230.0 MPa | T6 | Pink Sheets, ASTM B108, ASTM B955 | Casting | |||
24 °C | 227 MPa Show Material materials with Resistencia a la tracción of 227 MPa | T6 | Sand cast | |||
100 °C | 220 MPa Show Material materials with Resistencia a la tracción of 220 MPa | T6 | Sand cast | |||
150 °C | 160 MPa Show Material materials with Resistencia a la tracción of 160 MPa | T6 | Sand cast | |||
205 °C | 83 MPa Show Material materials with Resistencia a la tracción of 83 MPa | T6 | Sand cast | |||
260 °C | 53 MPa Show Material materials with Resistencia a la tracción of 53 MPa | T6 | Sand cast | |||
315 °C | 28 MPa Show Material materials with Resistencia a la tracción of 28 MPa | T6 | Sand cast | |||
371 °C | 17 MPa Show Material materials with Resistencia a la tracción of 17 MPa | T6 | Sand cast | |||
Resistencia al cizallamiento | 179 MPa Show Material materials with Resistencia al cizallamiento of 179 MPa | T6 |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Calor específico | 970.0 J/(kg·K) Show Material materials with Calor específico of 970.0 J/(kg·K) | T6 | ||||
100 °C | 960 J/(kg·K) Show Material materials with Calor específico of 960 J/(kg·K) | T6 | derived value | |||
Coeficiente de dilatación térmica | 2.2e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.2e-05 1/K | T6 | ||||
Conductividad térmica | 150.0 W/(m·K) Show Material materials with Conductividad térmica of 150.0 W/(m·K) | T6 | ||||
25 °C | 150 W/(m·K) Show Material materials with Conductividad térmica of 150 W/(m·K) | T6 | derived value | |||
Temperatura de fusión | 557.0 - 613.0 °C Show Material materials with Temperatura de fusión of 557.0 - 613.0 °C | T6 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955 | Casting | ||
570.0 °C Show Material materials with Temperatura de fusión of 570.0 °C | T6 |
Eléctrico
Property | Value | Condition | Comment |
---|---|---|---|
Conductividad eléctrica | 23000000 S/m Show Material materials with Conductividad eléctrica of 23000000 S/m | T6 | Typical/Derived values |
Resistividad eléctrica | 4.42e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.42e-08 Ω·m | T6 | Typical values |
Specific Electrical conductivity | 39.0 - 41.0 % IACS Show Material materials with Specific Electrical conductivity of 39.0 - 41.0 % IACS | T6 | Typical values |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminio | 90.1 - 93.3 % Show Material materials with Aluminio of 90.1 - 93.3 % | T6 | ||
Cobre | 0.25 % Show Material materials with Cobre of 0.25 % | T6 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955 | Casting |
Hierro | 0.6 % Show Material materials with Hierro of 0.6 % | T6 | ||
0.60 % Show Material materials with Hierro of 0.60 % | T6 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955 | Casting | |
Magnesio | 0.2 - 0.45 % Show Material materials with Magnesio of 0.2 - 0.45 % | T6 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955 | Casting |
Manganeso | 0.35 % Show Material materials with Manganeso of 0.35 % | T6 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955 | Casting |
Otro | 0.15 % Show Material materials with Otro of 0.15 % | T6 | ||
Silicona | 6.5 - 7.5 % Show Material materials with Silicona of 6.5 - 7.5 % | T6 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955 | Casting |
Titanio | 0.25 % Show Material materials with Titanio of 0.25 % | T6 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955 | Casting |
Zinc | 0.35 % Show Material materials with Zinc of 0.35 % | T6 | Pink Sheets, ASTM B108, ASTM B26, ASTM B618, ASTM B955 | Casting |