General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 7.8 g/cm³ Show Material materials with Densidad of 7.8 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Coeficiente de Poisson | 23.0 °C | 0.3 [-] Show Material materials with Coeficiente de Poisson of 0.3 [-] | Typical for Austenitic Stainless Steel |
Elongación | 23.0 °C | 23 % Show Material materials with Elongación of 23 % | |
Límite elástico | 23.0 °C | 480 MPa Show Material materials with Límite elástico of 480 MPa | |
Módulo de cizallamiento | 23.0 °C | 77 GPa Show Material materials with Módulo de cizallamiento of 77 GPa | Typical for Austenitic Stainless Steel |
Módulo elástico | 23.0 °C | 220 GPa Show Material materials with Módulo elástico of 220 GPa | |
Resistencia a la tracción | 23.0 °C | 790 MPa Show Material materials with Resistencia a la tracción of 790 MPa |
Aplicaciones térmicas
Property | Temperature | Value | Comment |
---|---|---|---|
Calor específico | 23.0 °C | 480 J/(kg·K) Show Material materials with Calor específico of 480 J/(kg·K) | |
Coeficiente de dilatación térmica | 23.0 °C | 1.6E-5 1/K Show Material materials with Coeficiente de dilatación térmica of 1.6E-5 1/K | |
Conductividad térmica | 23.0 °C | 13 W/(m·K) Show Material materials with Conductividad térmica of 13 W/(m·K) | |
Temperatura de fusión | 1230 - 1480 °C Show Material materials with Temperatura de fusión of 1230 - 1480 °C | Typical for Austenitic Stainless Steel |
Eléctrico
Property | Temperature | Value | Comment |
---|---|---|---|
Resistividad eléctrica | 23.0 °C | 8.5E-7 Ω·m Show Material materials with Resistividad eléctrica of 8.5E-7 Ω·m | Typical for Austenitic Stainless Steel |
Chemical properties
Property | Value |
---|---|
Azufre | 0 - 0.03 % Show Material materials with Azufre of 0 - 0.03 % |
Carbono | 0 - 0.06 % Show Material materials with Carbono of 0 - 0.06 % |
Cromo | 20.5 - 23.5 % Show Material materials with Cromo of 20.5 - 23.5 % |
Fósforo | 0 - 0.04 % Show Material materials with Fósforo of 0 - 0.04 % |
Hierro | 52.1 - 62.1 % Show Material materials with Hierro of 52.1 - 62.1 % |
Manganeso | 4 - 6 % Show Material materials with Manganeso of 4 - 6 % |
Molibdeno | 1.5 - 3 % Show Material materials with Molibdeno of 1.5 - 3 % |
Niobio | 0.1 - 0.3 % Show Material materials with Niobio of 0.1 - 0.3 % |
Nitrógeno | 0.2 - 0.4 % Show Material materials with Nitrógeno of 0.2 - 0.4 % |
Níquel | 11.5 - 13.5 % Show Material materials with Níquel of 11.5 - 13.5 % |
Silicona | 0 - 0.75 % Show Material materials with Silicona of 0 - 0.75 % |
Vanadio | 0.1 - 0.3 % Show Material materials with Vanadio of 0.1 - 0.3 % |