General
Property | Value | Thickness | Testing Standard | Condition | Comment |
---|---|---|---|---|---|
Absorción de agua | 0.2 % Show Supplier Material materials with Absorción de agua of 0.2 % | 2 mm | ISO 62 | 24h immersion at 23°C | |
Densidad | 1.62 g/cm³ Show Supplier Material materials with Densidad of 1.62 g/cm³ | ISO 1183 | dry |
Mecánica
Property | Temperature | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|---|
Elongación | 2 % Show Supplier Material materials with Elongación of 2 % | dry | ISO 527-2/1A | 5mm/min | |
Módulo de flexión | 15.5 GPa Show Supplier Material materials with Módulo de flexión of 15.5 GPa | dry | ISO 178 | 2mm/min | |
Módulo elástico | 18.1 GPa Show Supplier Material materials with Módulo elástico of 18.1 GPa | dry | ISO 527-2/1A | 1mm/min | |
Resistencia a la flexión | 360 MPa Show Supplier Material materials with Resistencia a la flexión of 360 MPa | dry | ISO 178 | 2mm/min | |
Resistencia a la tracción | 250 MPa Show Supplier Material materials with Resistencia a la tracción of 250 MPa | dry | ISO 527-2/1A | 5mm/min | |
Resistencia al choque, ensayo Charpy entallado | 23 °C | 16 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy entallado of 16 kJ/m² | dry | ISO 179/1eA | |
Resistencia al choque, ensayo Charpy no entallado | 23 °C | 80 kJ/m² Show Supplier Material materials with Resistencia al choque, ensayo Charpy no entallado of 80 kJ/m² | dry | ISO 179/1eU |
Aplicaciones térmicas
Property | Value | Thickness | Testing Standard | Comment | |||
---|---|---|---|---|---|---|---|
Temperatura de fusión | 310 °C Show Supplier Material materials with Temperatura de fusión of 310 °C | 1e+12 mm | ISO 11357-1/-3 | 10°C/min | |||
Inflamabilidad | Thickness tested (mm): 3 Class: HB, Standard: UL 94 |
Eléctrico
Property | Value | Condition | Testing Standard | Comment |
---|---|---|---|---|
Volume resistivity | 1e+13 Ω·cm Show Supplier Material materials with Volume resistivity of 1e+13 Ω·cm | dry | IEC 60093 | 500V |
Technological properties
Property | ||
---|---|---|
Additives | Release agent | |
Certifications | RoHS 2011/65/UE | |
Color | Black | |
Features | Heat Stabilized | |
Fillers | 50% Glass Fiber | |
Processing methods | Injection Molding |