UGI® 4539 is austenitic steel that is designed for high corrosion resistance, especially in Sulfuric Acid, in a wide range of process (chemical) environments. The combination of high chromium and nickel content, coupled with additions of molybdenum assure good to excellent corrosion resistance.


It has a fully austenitic micro structure.


This grade is non-magnetic in all conditions and has excellent Weldability and formability. The austenitic structure also gives this grade excellent toughness, even down to cryogenic temperatures.

Equivalent Materials

Los datos sobre este material han sido proporcionados por Ugitech SA.

A menos que se indique lo contrario, todas las medidas corresponden a condiciones de temperatura ambiente. A menos que se indique lo contrario, se utilizan las unidades del SI.
Las normas armonizadas son similares a uno o varios estándares del proveedor. Es posible que algunas normas armonizadas se ajusten al estándar original, mientras que otras pueden quedar fuera de su alcance.

Ashby charts

Propiedades

General

PropertyValue

Densidad

8 g/cm³

Show Supplier Material materials with Densidad of 8 g/cm³

Mecánica

PropertyTemperatureValueComment

Charpy impact energy, V-notch

100 J

Show Supplier Material materials with Charpy impact energy, V-notch of 100 J

min.

Dureza Brinell

230.0

Show Supplier Material materials with Dureza Brinell of 230.0

max.

Elongación

35 %

Show Supplier Material materials with Elongación of 35 %

Módulo elástico

100 °C

190 GPa

Show Supplier Material materials with Módulo elástico of 190 GPa

200 °C

180 GPa

Show Supplier Material materials with Módulo elástico of 180 GPa

300 °C

172 GPa

Show Supplier Material materials with Módulo elástico of 172 GPa

400 °C

165 GPa

Show Supplier Material materials with Módulo elástico of 165 GPa

500 °C

158 GPa

Show Supplier Material materials with Módulo elástico of 158 GPa

Resistencia a la tracción

530.0 - 730.0 MPa

Show Supplier Material materials with Resistencia a la tracción of 530.0 - 730.0 MPa

Aplicaciones térmicas

PropertyTemperatureValueComment

Calor específico

100 °C

485 J/(kg·K)

Show Supplier Material materials with Calor específico of 485 J/(kg·K)

200 °C

515 J/(kg·K)

Show Supplier Material materials with Calor específico of 515 J/(kg·K)

300 °C

545 J/(kg·K)

Show Supplier Material materials with Calor específico of 545 J/(kg·K)

400 °C

570 J/(kg·K)

Show Supplier Material materials with Calor específico of 570 J/(kg·K)

500 °C

590 J/(kg·K)

Show Supplier Material materials with Calor específico of 590 J/(kg·K)

Coeficiente de dilatación térmica

0.000014 1/K

Show Supplier Material materials with Coeficiente de dilatación térmica of 0.000014 1/K

20 to 100°C

0.000016 1/K

Show Supplier Material materials with Coeficiente de dilatación térmica of 0.000016 1/K

20 to 200°C

0.000018 1/K

Show Supplier Material materials with Coeficiente de dilatación térmica of 0.000018 1/K

20 to 300°C

0.00002 1/K

Show Supplier Material materials with Coeficiente de dilatación térmica of 0.00002 1/K

20 to 400°C

0.000022 1/K

Show Supplier Material materials with Coeficiente de dilatación térmica of 0.000022 1/K

20 to 500°C

Conductividad térmica

100 °C

14 W/(m·K)

Show Supplier Material materials with Conductividad térmica of 14 W/(m·K)

200 °C

16 W/(m·K)

Show Supplier Material materials with Conductividad térmica of 16 W/(m·K)

300 °C

18 W/(m·K)

Show Supplier Material materials with Conductividad térmica of 18 W/(m·K)

400 °C

20 W/(m·K)

Show Supplier Material materials with Conductividad térmica of 20 W/(m·K)

500 °C

22 W/(m·K)

Show Supplier Material materials with Conductividad térmica of 22 W/(m·K)

Eléctrico

PropertyTemperatureValue

Resistividad eléctrica

100 °C

0.00000099 Ω·m

Show Supplier Material materials with Resistividad eléctrica of 0.00000099 Ω·m

200 °C

0.00000107 Ω·m

Show Supplier Material materials with Resistividad eléctrica of 0.00000107 Ω·m

300 °C

0.00000113 Ω·m

Show Supplier Material materials with Resistividad eléctrica of 0.00000113 Ω·m

400 °C

0.00000115 Ω·m

Show Supplier Material materials with Resistividad eléctrica of 0.00000115 Ω·m

500 °C

0.00000117 Ω·m

Show Supplier Material materials with Resistividad eléctrica of 0.00000117 Ω·m

Chemical properties

PropertyValueComment

Azufre

0.015

Show Supplier Material materials with Azufre of 0.015

max.

Carbono

0.02

Show Supplier Material materials with Carbono of 0.02

max.

Cobre

1.0 - 2.0 %

Show Supplier Material materials with Cobre of 1.0 - 2.0 %

Cromo

19.0 - 21.0 %

Show Supplier Material materials with Cromo of 19.0 - 21.0 %

Fósforo

0.035

Show Supplier Material materials with Fósforo of 0.035

max.

Manganeso

2.0

Show Supplier Material materials with Manganeso of 2.0

max.

Molibdeno

4.0 - 5.0 %

Show Supplier Material materials with Molibdeno of 4.0 - 5.0 %

Nitrógeno

0.1

Show Supplier Material materials with Nitrógeno of 0.1

max.

Níquel

23.0 - 28.0 %

Show Supplier Material materials with Níquel of 23.0 - 28.0 %

Silicona

0.7000000000000001

Show Supplier Material materials with Silicona of 0.7000000000000001

max.

Technological properties

Property
Application areas

  • Chemical and petrochemical industries
  • Sulfuric acid handling devices
  • Wrist watch and jewelry components
  • Medical and pharmaceutical applications
  • Pulp and paper industry
  • Cold Forming

    UGI® 4539 is quite ductile and forms easily. The high strength of the high nitrogen and molybdenum containing UGI® 4539 is clearly demonstrated when the stress-strain curves of this grades is compared with the standard austenitic product 304/304L grades.

    Corrosion properties

    Although originally developed for its uniform corrosion resistance to sulphuric acid, it also has a very high resistance to a wide range of environments. Its value of PREN* between 33 and 38 indicates that the material has good pitting corrosion resistance to warm sea water and other high chloride environments.


    Uniform corrosion: Uniform corrosion occurs when all of the passive layer is destroyed. This typically occurs in acids or in hot alkaline solutions. The table below gives for different solutions the limit in temperature for a corrosion rate < 0,1 mm/year:


    Acid or alkaline concentration
    Weight %
    H₂SO₄
    20%
    H₂SO₄
    40%
    H₂SO₄
    60%
    HCL
    1%
    HCL
    2%
    HCL
    3%
    NaOH
    20%
    NaOH
    40%
    NaOH
    60%
    Temperature limit* in °C (< 0.1 mm /y)70°C55°C40°C60°C30°C20°C170°C125°C160°C

    *The temperature limit can be influenced too by the surface: roughness …


    Localized corrosion

    Pitting corrosion: Chloride ions in a neutral or acidic environment facilitate local breakdown of the passive layer. As a result, pitting and crevice corrosion can propagate, causing corrosion failures. The PREN value can be used for rough comparisons of different grades. A more reliable means, however, is to rank the grades according to the critical pitting temperature (CPT). There are several different methods available, for example ASTMG 150 with a 1M NaCl solution (35 000 ppm chloride ions). The CPT values are shown in the table below:


    GradeUGI 4404UGI® 4539UGI 4462
    CPT* in°C (ASTM G150)18°C60°C50°C

    *(%Cr+3.3*%Mo+16*%N) **The CPT can be influenced too by the surface: roughness …


    Intergranular corrosion: UGI® 4539 has very low carbon content. This means that there is very little risk of carbide precipitation in connection with ordinary heat treatment and welding. The risk of intergranular corrosion after ordinary heat treatment and welding is thereby eliminated.


    Stress corrosion: Owing to its high nickel and molybdenum contents, UGI® 4539 is highly resistant to stress corrosion cracking in chloride solutions, or concentrated hydroxide solutions and in environments rich in hydrogen sulphide (oil and gas market). The graph below represents for different grades the range of cracking resistance in function of temperature and H₂S pressure: the limit for UGI® 4539 is in blue on the graph on the right side of the material page.

    General machinability

    Like other austenitic steels, UGI® 4539 is tough and is prone to develop cold work-hardening. Moreover its sulphur content is kept low. All of that makes it less machinable than 410 and 304 grades. However with the right choice of tool and machine data, fully satisfactory machining results can be obtained on it.

    Heat Treatment

    Solution annealing

    Optimal mechanical and fabrication properties are realized after solution annealing in the temperature range 1060°C – 1150°C followed by rapid cooling in air or water. Exposure to temperatures in the range 600°C – 900°C must be minimized to prevent the formation of brittle and less corrosion resistant intermetallic phases.

    Hardening

    UGI® 4539 cannot be hardened by heat treatment but it can be hardened by cold working.

    Hot forming

    Forging

    UGI® 4539 is usually pre-heated to between 1150 – 1180°C with forging taking place between 1180 and 950°C. After forging, the forged component must be rapidly cooled in air or in water when no danger of distortion exists.

    Other

    Available products:


    ProductFormFinitionToleranceDimension


    Bars
    RoundDrawnh92-28 mm
    RoundGroundh7-h92-80 mm
    RoundTurned and polishedh10-h1122-130 mm
    RoundDescaledk12-k1322-130 mm
    HexagonalDrawn3-55 mm
    Wire rodRoundPickled5-32 mm
    Drawn wireRoundMat0.8-14 mm
    ProfileBright2-70 m²


    Other formats: contact the supplier

    Surface Treatment

    Pickling

    This process is necessary when oxidized surfaces are present during heating. An acid bath must be used: hydrochloric acid, or sulphuric acid, or mixed nitro-hydrofluoric acids. Warming the bath (e.g. to 50°C) reduces immersion time. Finally, it is absolutely essential to rinse the surfaces thoroughly.


    Passivation

    Stainless steels, especially those with high Chromium/Molybdenum content, do not generally need to be passivated as the passive film forms spontaneously in air and, after 24 hours, it achieves a certain stability. On the other hand, stainless steels can be contaminated by contact with carbon steels or low-alloy steels: this phenomenon is known as ferrous contamination. In this case, nitric acid passivation for 30 minutes at ambient temperature is required. Surface rinsing or even surface neutralization is essential as a final treatment.


    Electropolishing

    The usual molybdenum austenitic steel electropolishing conditions can be used for UGI® 4539

    Welding

    UGI® 4539 during welding displays a tendency towards hot cracking due to its full austenitic solidification structure. Nevertheless it is readily weldable using all standard welding processes on SS Austenitics. Welding without the use of a filler metal is not recommended since this will promote the tendency for hot crack formation. When using matching filler materials, care must be taken to limit the heat input to low values which could result in poor fusion.

    Weaving during welding must also be avoided in order to minimize the heat input. Heat treatment after welding is not necessary, and even large sections are resistant to inter-crystalline corrosion after welding, due to the low carbon content.