General
Property | Value |
---|---|
Densidad | 7.8 g/cm³ Show Supplier Material materials with Densidad of 7.8 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Dureza Brinell | 375.0 [-] Show Supplier Material materials with Dureza Brinell of 375.0 [-] | min. | |
Dureza Rockwell C | 38.0 [-] Show Supplier Material materials with Dureza Rockwell C of 38.0 [-] | min. | |
Elongación | 10 % Show Supplier Material materials with Elongación of 10 % | min. | |
Estricción | 44.0 % Show Supplier Material materials with Estricción of 44.0 % | min. | |
Módulo elástico | 20 °C | 200 GPa Show Supplier Material materials with Módulo elástico of 200 GPa | |
100 °C | 195 GPa Show Supplier Material materials with Módulo elástico of 195 GPa | ||
200 °C | 185 GPa Show Supplier Material materials with Módulo elástico of 185 GPa | ||
300 °C | 170 GPa Show Supplier Material materials with Módulo elástico of 170 GPa | ||
300 °C | 175 GPa Show Supplier Material materials with Módulo elástico of 175 GPa | ||
Resistencia a la tracción | 1170 MPa Show Supplier Material materials with Resistencia a la tracción of 1170 MPa | min. |
Aplicaciones térmicas
Property | Value | Comment |
---|---|---|
Calor específico | 500 J/(kg·K) Show Supplier Material materials with Calor específico of 500 J/(kg·K) | |
Coeficiente de dilatación térmica | 0.0000105 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 0.0000105 1/K | 20 to 100°C |
0.0000111 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 0.0000111 1/K | 20 to 200°C | |
0.0000115 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 0.0000115 1/K | 20 to 300°C | |
0.0000119 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 0.0000119 1/K | 20 to 400°C | |
Conductividad térmica | 16 W/(m·K) Show Supplier Material materials with Conductividad térmica of 16 W/(m·K) |
Eléctrico
Property | Value |
---|---|
Resistividad eléctrica | 7.1e-07 Ω·m Show Supplier Material materials with Resistividad eléctrica of 7.1e-07 Ω·m |
Chemical properties
Property | Value | Comment |
---|---|---|
Azufre | 0.005 Show Supplier Material materials with Azufre of 0.005 | max. |
Carbono | 0.07 Show Supplier Material materials with Carbono of 0.07 | max. |
Cobre | 2.5 - 4.0 % Show Supplier Material materials with Cobre of 2.5 - 4.0 % | |
Cromo | 14.5 - 15.3 % Show Supplier Material materials with Cromo of 14.5 - 15.3 % | |
Fósforo | 0.025 Show Supplier Material materials with Fósforo of 0.025 | max. |
Manganeso | 1.0 Show Supplier Material materials with Manganeso of 1.0 | max. |
Molibdeno | 0.5 Show Supplier Material materials with Molibdeno of 0.5 | max. |
Niobio | 0.45 Show Supplier Material materials with Niobio of 0.45 | max., min: 5xC |
Níquel | 4.5 - 5.5 % Show Supplier Material materials with Níquel of 4.5 - 5.5 % | |
Silicona | 0.6000000000000001 Show Supplier Material materials with Silicona of 0.6000000000000001 | max. |
Technological properties
Property | ||
---|---|---|
Application areas | UGI®15-5 PH AIR is suitable for | |
Corrosion properties | UGI®15-5 PH AIR offers good corrosion resistance, sometimes similar to that of type 18 Cr-8Ni austenitic steels in some cases. | |
General machinability | Because of its low sulphur content and its very good micro-cleanliness, UGI®15-5 PH AIR has a poor chip breakability which can induce difficulties during machining, especially in drilling or finish turning operations. If possible, most of the machining operations to obtain the final parts have to be done in the A-condition (solution annealed) state in order to avoid too important tool wears during machining. Machining after a “precipitation hardening” heat treatment is not recommended because the higher the mechanical characteristics of the UGI®15-5 PH AIR bars to be machined, the higher the tool wears (and thus the lower the machining productivity). In A-condition, rough turning tests (ap = 1.5 mm; f = 0.25 mm/rev) performed on drawn bars have shown that the cutting speed to have a flank wear of 0.15 mm in 15 min of effective cutting with a STELLRAM SP4019 CCGT 09T308E-62 tool is ~ 145 m/min whereas that of a UGIMA®4542 (17-4 PH with improved machinability) is ~ 160 m/min. Depending on the machining operation, the machining productivity of UGI®15-5 PH AIR is found to be 10 to 30% lower than UGIMA® 4542. | |
Heat Treatment | Heat treatments carried out on UGI®15-5PH AIR are composed of two steps: Austenitisation: Solution annealing is performed around 1030-1050°C, and is interrupted by oil quenching or alternatively by air cooling for small section parts. In this condition (called condition A) hardness is intermediate because Cu precipitation hardening is not effective. Hence, the A-condition is often chosen to carry out machining or cold forming operations. In that case, we recommend performing a stress relief treatment at 300°C for 1 hour after austenitisation, in order to stabilize the material and avoid quench-cracking issues. Aging: Aging treatments are performed after solution treatment to make Cu rich phases precipitate and adjust me-chanical properties. After aging, the material is in the solution and aged condition, also called H-condition. Aging treatments can be performed between 480°C (condition H900) and 620°C (condition H1150). The condition H900 corresponds to the peak of hardening, for which the Cu precipitates induce a maximum of hardness. For higher temperature the hardness/strength decreases when increasing aging temperature, due to the growth of the precipitates. Beyond 580°C some reverted austenite is formed during the aging which results in an increase of the toughness but a drop of the strength. The condition H1025 is often chosen by customers because it leads to an optimal trade-off between strength and toughness. Softening: The lowest strength or hardness is obtained after the thermal cycle H1150M, consisting into of a solution an-nealing followed by a tempering at 760°C for 2 hours and an aging at 620°C for 4 hours. After this heat treatment cycle the mechanical properties are UTS = 780 MPa, YS = 710 MPa, HRC < 32 HRC, which is sig-nificantly lower than the condition A. | |
Hot forming | UGI®15-5 PH AIR is suitable for forging. Reheating must be carried out at a temperature between 1150 and 1200°C, forging between 1200°C and 950°C. Cooling after forging must be performed in air or oil. The parts obtained in this way have to be heat treated (solution annealing and eventual aging, see previous section) | |
Other | Magnetic particle inspection and macro-graph UGI®15-5 PH AIR complies with AMS 2300: Frequency/Severity rating 0/0 Macrostructure of UGI®15-5PH AIR is conforming to AMS 5659: class 1 to 4 are generally quoted severity A according to ASTM A604. Available products: Other products: contact the supplier | |
Surface Treatment | Pickling procedure: UGI®15-5 PH AIR is pickled in the same way as 630 grade steel. | |
Welding | UGI®15-5 PH AIR can be welded without preheating, using most welding techniques: GMAW or GTAW (with or without filler wire), LASER, resistance or electron beam welding, etc. If the mechanical characteristics of the weld area have to be at the same level as that of the base metal, no filler metal or homogeneous filler metal (such as AWS E/ER 630) have to be used and a post weld heat treatment of precipitation hardening (see the different PH heat treatment on page 4) has to be performed on the weld. If the mechanical characteristics of the weld area does not have to be at the same level as that of the base metal, a filler metal such as ER308LSi (19 9 L Si) can be used. If no precipitation hardening heat treatment is done after welding, a stress relief heat treatment at 250/300°C could be useful to increase the toughness of the HAZ and avoid any risk of cold cracking due to their as-welded martensitic microstructures. Furthermore, it should be restated that the welding design should make allowance for the care required with all high steels with high proof stress: avoiding cut outs and sudden changes in cross section. For GMAW, we recommend the use of a protective gas made up of Ar+1%CO₂ or 1-2%O₂; for GMAW as well as for GTAW, gasses containing H₂ and N₂ must be avoided. |