General
Property | Temperature | Value |
---|---|---|
Densidad | 23.0 °C | 8 g/cm³ Show Supplier Material materials with Densidad of 8 g/cm³ |
Mecánica
Property | Temperature | Value | Comment |
---|---|---|---|
Dureza Brinell | 23.0 °C | 210 [-] Show Supplier Material materials with Dureza Brinell of 210 [-] | max. |
Elongación A5 | 23.0 °C | 30 % Show Supplier Material materials with Elongación A5 of 30 % | for 20 to 800°C |
Límite elástico Rp 0,2 | 20.0 °C | 285 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 285 MPa | |
100.0 °C | 265 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 265 MPa | ||
200.0 °C | 240 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 240 MPa | ||
300.0 °C | 220 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 220 MPa | ||
400.0 °C | 210 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 210 MPa | ||
500.0 °C | 200 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 200 MPa | ||
600.0 °C | 195 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 195 MPa | ||
700.0 °C | 175 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 175 MPa | ||
800.0 °C | 135 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 135 MPa | ||
900.0 °C | 85 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 85 MPa | ||
1000.0 °C | 48 MPa Show Supplier Material materials with Límite elástico Rp 0,2 of 48 MPa | ||
Límite elástico Rp 1,0 | 20.0 °C | 310 MPa Show Supplier Material materials with Límite elástico Rp 1,0 of 310 MPa | |
100.0 °C | 290 MPa Show Supplier Material materials with Límite elástico Rp 1,0 of 290 MPa | ||
200.0 °C | 265 MPa Show Supplier Material materials with Límite elástico Rp 1,0 of 265 MPa | ||
300.0 °C | 250 MPa Show Supplier Material materials with Límite elástico Rp 1,0 of 250 MPa | ||
400.0 °C | 235 MPa Show Supplier Material materials with Límite elástico Rp 1,0 of 235 MPa | ||
500.0 °C | 225 MPa Show Supplier Material materials with Límite elástico Rp 1,0 of 225 MPa | ||
600.0 °C | 215 MPa Show Supplier Material materials with Límite elástico Rp 1,0 of 215 MPa | ||
700.0 °C | 190 MPa Show Supplier Material materials with Límite elástico Rp 1,0 of 190 MPa | ||
800.0 °C | 145 MPa Show Supplier Material materials with Límite elástico Rp 1,0 of 145 MPa | ||
900.0 °C | 100 MPa Show Supplier Material materials with Límite elástico Rp 1,0 of 100 MPa | ||
1000.0 °C | 55 MPa Show Supplier Material materials with Límite elástico Rp 1,0 of 55 MPa | ||
Módulo elástico | -100.0 °C | 201 GPa Show Supplier Material materials with Módulo elástico of 201 GPa | |
0.0 °C | 196 GPa Show Supplier Material materials with Módulo elástico of 196 GPa | ||
20.0 °C | 194 GPa Show Supplier Material materials with Módulo elástico of 194 GPa | ||
100.0 °C | 189 GPa Show Supplier Material materials with Módulo elástico of 189 GPa | ||
200.0 °C | 183 GPa Show Supplier Material materials with Módulo elástico of 183 GPa | ||
300.0 °C | 177 GPa Show Supplier Material materials with Módulo elástico of 177 GPa | ||
400.0 °C | 170 GPa Show Supplier Material materials with Módulo elástico of 170 GPa | ||
500.0 °C | 163 GPa Show Supplier Material materials with Módulo elástico of 163 GPa | ||
600.0 °C | 156 GPa Show Supplier Material materials with Módulo elástico of 156 GPa | ||
700.0 °C | 149 GPa Show Supplier Material materials with Módulo elástico of 149 GPa | ||
800.0 °C | 141 GPa Show Supplier Material materials with Módulo elástico of 141 GPa | ||
900.0 °C | 134 GPa Show Supplier Material materials with Módulo elástico of 134 GPa | ||
1000.0 °C | 127 GPa Show Supplier Material materials with Módulo elástico of 127 GPa | ||
Resistencia a la tracción | 20.0 °C | 650 MPa Show Supplier Material materials with Resistencia a la tracción of 650 MPa | |
100.0 °C | 630 MPa Show Supplier Material materials with Resistencia a la tracción of 630 MPa | ||
200.0 °C | 615 MPa Show Supplier Material materials with Resistencia a la tracción of 615 MPa | ||
300.0 °C | 605 MPa Show Supplier Material materials with Resistencia a la tracción of 605 MPa | ||
400.0 °C | 590 MPa Show Supplier Material materials with Resistencia a la tracción of 590 MPa | ||
500.0 °C | 555 MPa Show Supplier Material materials with Resistencia a la tracción of 555 MPa | ||
600.0 °C | 480 MPa Show Supplier Material materials with Resistencia a la tracción of 480 MPa | ||
700.0 °C | 340 MPa Show Supplier Material materials with Resistencia a la tracción of 340 MPa | ||
800.0 °C | 210 MPa Show Supplier Material materials with Resistencia a la tracción of 210 MPa | ||
900.0 °C | 120 MPa Show Supplier Material materials with Resistencia a la tracción of 120 MPa | ||
1000.0 °C | 80 MPa Show Supplier Material materials with Resistencia a la tracción of 80 MPa | ||
Aplicaciones térmicas
Property | Temperature | Value |
---|---|---|
Calor específico | -100.0 °C | 394 J/(kg·K) Show Supplier Material materials with Calor específico of 394 J/(kg·K) |
0.0 °C | 467 J/(kg·K) Show Supplier Material materials with Calor específico of 467 J/(kg·K) | |
20.0 °C | 472 J/(kg·K) Show Supplier Material materials with Calor específico of 472 J/(kg·K) | |
100.0 °C | 501 J/(kg·K) Show Supplier Material materials with Calor específico of 501 J/(kg·K) | |
200.0 °C | 525 J/(kg·K) Show Supplier Material materials with Calor específico of 525 J/(kg·K) | |
300.0 °C | 532 J/(kg·K) Show Supplier Material materials with Calor específico of 532 J/(kg·K) | |
400.0 °C | 555 J/(kg·K) Show Supplier Material materials with Calor específico of 555 J/(kg·K) | |
500.0 °C | 582 J/(kg·K) Show Supplier Material materials with Calor específico of 582 J/(kg·K) | |
600.0 °C | 604 J/(kg·K) Show Supplier Material materials with Calor específico of 604 J/(kg·K) | |
700.0 °C | 610 J/(kg·K) Show Supplier Material materials with Calor específico of 610 J/(kg·K) | |
800.0 °C | 609 J/(kg·K) Show Supplier Material materials with Calor específico of 609 J/(kg·K) | |
900.0 °C | 615 J/(kg·K) Show Supplier Material materials with Calor específico of 615 J/(kg·K) | |
1000.0 °C | 641 J/(kg·K) Show Supplier Material materials with Calor específico of 641 J/(kg·K) | |
Coeficiente de dilatación térmica | -100.0 °C | 1.36E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.36E-5 1/K |
100.0 °C | 1.51E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.51E-5 1/K | |
200.0 °C | 1.57E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.57E-5 1/K | |
300.0 °C | 1.62E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.62E-5 1/K | |
400.0 °C | 1.66E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.66E-5 1/K | |
500.0 °C | 1.7E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.7E-5 1/K | |
600.0 °C | 1.74E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.74E-5 1/K | |
700.0 °C | 1.77E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.77E-5 1/K | |
800.0 °C | 1.8E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.8E-5 1/K | |
900.0 °C | 1.83E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.83E-5 1/K | |
1000.0 °C | 1.86E-5 1/K Show Supplier Material materials with Coeficiente de dilatación térmica of 1.86E-5 1/K | |
Conductividad térmica | 20.0 °C | 11.4 W/(m·K) Show Supplier Material materials with Conductividad térmica of 11.4 W/(m·K) |
100.0 °C | 12.8 W/(m·K) Show Supplier Material materials with Conductividad térmica of 12.8 W/(m·K) | |
200.0 °C | 14.6 W/(m·K) Show Supplier Material materials with Conductividad térmica of 14.6 W/(m·K) | |
300.0 °C | 16.3 W/(m·K) Show Supplier Material materials with Conductividad térmica of 16.3 W/(m·K) | |
400.0 °C | 17.9 W/(m·K) Show Supplier Material materials with Conductividad térmica of 17.9 W/(m·K) | |
500.0 °C | 19.5 W/(m·K) Show Supplier Material materials with Conductividad térmica of 19.5 W/(m·K) | |
600.0 °C | 21 W/(m·K) Show Supplier Material materials with Conductividad térmica of 21 W/(m·K) | |
700.0 °C | 22.6 W/(m·K) Show Supplier Material materials with Conductividad térmica of 22.6 W/(m·K) | |
800.0 °C | 24.1 W/(m·K) Show Supplier Material materials with Conductividad térmica of 24.1 W/(m·K) | |
900.0 °C | 25.6 W/(m·K) Show Supplier Material materials with Conductividad térmica of 25.6 W/(m·K) | |
1000.0 °C | 27 W/(m·K) Show Supplier Material materials with Conductividad térmica of 27 W/(m·K) | |
Temperatura de fusión | 1330 - 1400 °C Show Supplier Material materials with Temperatura de fusión of 1330 - 1400 °C |
Eléctrico
Property | Temperature | Value |
---|---|---|
Resistividad eléctrica | 20.0 °C | 1.04E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.04E-6 Ω·m |
100.0 °C | 1.07E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.07E-6 Ω·m | |
200.0 °C | 1.11E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.11E-6 Ω·m | |
300.0 °C | 1.14E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.14E-6 Ω·m | |
400.0 °C | 1.17E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.17E-6 Ω·m | |
500.0 °C | 1.19E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.19E-6 Ω·m | |
600.0 °C | 1.22E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.22E-6 Ω·m | |
700.0 °C | 1.23E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.23E-6 Ω·m | |
800.0 °C | 1.25E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.25E-6 Ω·m | |
900.0 °C | 1.27E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.27E-6 Ω·m | |
1000.0 °C | 1.29E-6 Ω·m Show Supplier Material materials with Resistividad eléctrica of 1.29E-6 Ω·m | |
Magnético
Property | Temperature | Value |
---|---|---|
Permeabilidad magnética relativa | 23.0 °C | 1.01 [-] Show Supplier Material materials with Permeabilidad magnética relativa of 1.01 [-] |
Chemical properties
Property | Value | Comment | |
---|---|---|---|
Azufre | 0.03 % Show Supplier Material materials with Azufre of 0.03 % | max. | |
Carbono | 0.1 % Show Supplier Material materials with Carbono of 0.1 % | max. | |
Cobre | 0.5 % Show Supplier Material materials with Cobre of 0.5 % | max. | |
Cromo | 17 - 19 % Show Supplier Material materials with Cromo of 17 - 19 % | ||
Fósforo | 0.03 % Show Supplier Material materials with Fósforo of 0.03 % | max. | |
Hierro | Balance | ||
Manganeso | 0.8 - 1.5 % Show Supplier Material materials with Manganeso of 0.8 - 1.5 % | ||
Níquel | 35 - 39 % Show Supplier Material materials with Níquel of 35 - 39 % | ||
Silicona | 1.9 - 2.5 % Show Supplier Material materials with Silicona of 1.9 - 2.5 % | ||
Titanio | 0.2 % Show Supplier Material materials with Titanio of 0.2 % | max. |
Technological properties
Property | ||
---|---|---|
Application areas | Nicrofer 3718 finds wide application in high-temperature processes: fans operating at high temperatures in carburising furnaces resisting carburisation, boxes and baskets used in carburising resisting carburisation and showing weight savings when compared with cast boxes, hangers, hooks and conveyor chains used to carry vitreous-enamelled components during firing resisting oxide spalling so that oxide does not fall on the enamel, combustion tubes resisting oxidation to carburisation and alternating oxidising and carburising conditions, jigs and fixtures used in furnace brazing and wire mesh belts to carry components in heat-treatment processes, thermocouple sheaths resisting carburisation and nitriding, flare-stack tips resisting alternating conditions, components handling cracked ammonia. | |
Cold Forming | Cold working should be carried out on annealed material. Nicrofer 3718 So* has a similar work-hardening rate compared to austenitic stainless steel and the forming equipment must be adapted accordingly. When cold working is performed, interstage annealing may become necessary. After cold reduction of more than 15%, final annealing is required before use, in so far as the creep-strength is important. Bending property and formability is given even with oxidised sheets. Nevertheless the bending radius should be 3 times sheet thickness. | |
Corrosion properties | The nickel-chromium-iron alloy Nicrofer 3718 So* containing about 2% silicon is a general-purpose heat-resisting material. They have good oxidation resistance up to about 1000 °C, particularly under cyclic conditions of heating and cooling. It also has excellent resistance to carburisation and are widely used in industry under such conditions. Its resistance to nitrogen-containing atmospheres where oxygen content is low makes them suitable for environments such as cracked ammonia. Due to its higher chromium and silicon contents, Nicrofer 3718 So* is in every respect superior to the standard alloy Nicrofer 3718. | |
General machinability | Nicrofer 3718 So* should be machined in the annealed condition. As the alloy is susceptible to work-hardening, a low cutting speed should be used and tools should be engaged at all times. Heavy feeds are important in betting below the work-hardened 'skin'. | |
Heat Treatment | Annealing should be carried out in the temperature range 1020 to 1120°C (1870 to 2050°F). Water quenching is essential for maximum creep resistance. During any heating operation, the precautions outlined earlier regarding cleanliness must be observed. | |
Hot forming | Nicrofer 3718 So* may be hot-worked in the range 1150 to 950 °C (2100 to 1740 °F). Cooling should be by water quenching or as fast as possible. Annealing is recommended after hot working to ensure maximum corrosion resistance and optimum structure. The material may be charged into the furnace at maximum working temperature. | |
Other | Nicrofer 3718 So* is a solid solution alloy with small amounts of precipitated titanium nitride and carbide as well as carbonitrides in the austenitic matrix. | |
Welding | Nicrofer 3718 So* can be welded by GTAW, plasma arc and SMAW processes. Prior to welding, material should be in the annealed condition, clean and free from scale, grease, marking paints etc. A zone approximately 25 mm (1 in) wide on each side of the joint should be ground to bright metal. Interpass temperature should not exceed 150°C (300°F). Neither pre- nor post-weld heat treatment is required. |