General
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Densidad | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 2.73 g/cm³ Show Material materials with Densidad of 2.73 g/cm³ | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube |
Mecánica
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Coeficiente de Poisson | 20.0 °C | 0.33 [-] Show Material materials with Coeficiente de Poisson of 0.33 [-] | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | |
Dureza Brinell | 51.0 [-] Show Material materials with Dureza Brinell of 51.0 [-] | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 47.0 [-] Show Material materials with Dureza Brinell of 47.0 [-] | H16 | EN 573-3 | Rod, Tube | ||
20.0 °C | 51.0 [-] Show Material materials with Dureza Brinell of 51.0 [-] | H16 | EN 573-3 | Flat | ||
Elongación | 1.0 % Show Material materials with Elongación of 1.0 % | H16 | EN 573-3, EN 485, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | |
2.0 % Show Material materials with Elongación of 2.0 % | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
3.0 % Show Material materials with Elongación of 3.0 % | H16 | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
3.0 % Show Material materials with Elongación of 3.0 % | H16 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
4.0 % Show Material materials with Elongación of 4.0 % | H16 | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | H16 | EN 573-3 | Foil, Flat | A50 | |
20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | H16 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 1.0 % Show Material materials with Elongación of 1.0 % | H16 | EN 573-3 | Foil | A100 | |
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | H16 | EN 573-3 | Flat | A50 | |
20.0 °C | 2.0 % Show Material materials with Elongación of 2.0 % | H16 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | H16 | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 3.0 % Show Material materials with Elongación of 3.0 % | H16 | EN 573-3 | Seamless Tube | ||
20.0 °C | 4.0 % Show Material materials with Elongación of 4.0 % | H16 | EN 573-3 | Rod, Tube | ||
Módulo de cizallamiento | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 24.0 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.5 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
20.0 °C | 24.0 - 26.1 GPa Show Material materials with Módulo de cizallamiento of 24.0 - 26.1 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
20.0 °C | 26.1 - 26.5 GPa Show Material materials with Módulo de cizallamiento of 26.1 - 26.5 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
20.0 °C | 26.1 GPa Show Material materials with Módulo de cizallamiento of 26.1 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
Módulo elástico | -270.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | |
69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 69.0 - 70.0 GPa Show Material materials with Módulo elástico of 69.0 - 70.0 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
20.0 °C | 69.0 - 69.5 GPa Show Material materials with Módulo elástico of 69.0 - 69.5 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
20.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
20.0 °C | 69.5 - 70.0 GPa Show Material materials with Módulo elástico of 69.5 - 70.0 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
20.0 °C | 69.5 GPa Show Material materials with Módulo elástico of 69.5 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
20.0 °C | 70.0 GPa Show Material materials with Módulo elástico of 70.0 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
50.0 °C | 69.0 GPa Show Material materials with Módulo elástico of 69.0 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
100.0 °C | 68.0 GPa Show Material materials with Módulo elástico of 68.0 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
150.0 °C | 66.0 GPa Show Material materials with Módulo elástico of 66.0 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
200.0 °C | 63.0 GPa Show Material materials with Módulo elástico of 63.0 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
250.0 °C | 57.0 GPa Show Material materials with Módulo elástico of 57.0 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
300.0 °C | 50.0 GPa Show Material materials with Módulo elástico of 50.0 GPa | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Resistencia a la tracción | 150.0 - 200.0 MPa Show Material materials with Resistencia a la tracción of 150.0 - 200.0 MPa | H16 | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
170.0 MPa Show Material materials with Resistencia a la tracción of 170.0 MPa | H16 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 150.0 - 190.0 MPa Show Material materials with Resistencia a la tracción of 150.0 - 190.0 MPa | H16 | EN 573-3 | Foil | ||
20.0 °C | 160.0 - 195.0 MPa Show Material materials with Resistencia a la tracción of 160.0 - 195.0 MPa | H16 | EN 573-3, EN 754 | Rod, Tube, Strip, Sheet, Plate, Foil, Bar | ||
20.0 °C | 160.0 - 200.0 MPa Show Material materials with Resistencia a la tracción of 160.0 - 200.0 MPa | H16 | EN 573-3, EN 485, EN 683 | Foil, Flat, Strip, Sheet, Plate, Bar, Rod, Tube | ||
20.0 °C | 160.0 - 200.0 MPa Show Material materials with Resistencia a la tracción of 160.0 - 200.0 MPa | H16 | EN 573-3 | Flat | Transverse | |
20.0 °C | 170.0 MPa Show Material materials with Resistencia a la tracción of 170.0 MPa | H16 | EN 573-3 | Seamless Tube | ||
Ángulo de flexión a 180° | 2.0 °/t Show Material materials with Ángulo de flexión a 180° of 2.0 °/t | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
2.5 °/t Show Material materials with Ángulo de flexión a 180° of 2.5 °/t | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
Ángulo de flexión a 90° | 1.0 °/t Show Material materials with Ángulo de flexión a 90° of 1.0 °/t | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
1.5 °/t Show Material materials with Ángulo de flexión a 90° of 1.5 °/t | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
2.0 °/t Show Material materials with Ángulo de flexión a 90° of 2.0 °/t | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Aplicaciones térmicas
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Calor específico | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 892.0 - 893.0 J/(kg·K) Show Material materials with Calor específico of 892.0 - 893.0 J/(kg·K) | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | |
20.0 °C | 892.0 J/(kg·K) Show Material materials with Calor específico of 892.0 J/(kg·K) | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | |
20.0 °C | 893.0 J/(kg·K) Show Material materials with Calor específico of 893.0 J/(kg·K) | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | |
Coeficiente de dilatación térmica | 20 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
100 °C | 2.35e-05 1/K Show Material materials with Coeficiente de dilatación térmica of 2.35e-05 1/K | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Conductividad térmica | 20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 - 200.0 W/(m·K) | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Seamless Tube |
20.0 °C | 160.0 W/(m·K) Show Material materials with Conductividad térmica of 160.0 W/(m·K) | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | |
Temperatura de fusión | 645.0 - 655.0 °C Show Material materials with Temperatura de fusión of 645.0 - 655.0 °C | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Eléctrico
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Conductividad eléctrica | 20.0 °C | 22000000.0 - 28000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 28000000.0 S/m | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Seamless Tube |
20.0 °C | 22000000.0 - 29000000.0 S/m Show Material materials with Conductividad eléctrica of 22000000.0 - 29000000.0 S/m | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | |
Resistividad eléctrica | 3.57e-08 - 4.55e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.57e-08 - 4.55e-08 Ω·m | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 3.4e-08 - 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.1e-08 Ω·m | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | |
20.0 °C | 3.4e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 3.4e-08 - 4.5e-08 Ω·m | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | |
20.0 °C | 4.1e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 Ω·m | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | |
20.0 °C | 4.1e-08 - 4.5e-08 Ω·m Show Material materials with Resistividad eléctrica of 4.1e-08 - 4.5e-08 Ω·m | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Cobre | 0.1 % Show Material materials with Cobre of 0.1 % | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Seamless Tube, Tube, Strip, Sheet, Plate, Bar |
Cromo | 0.1 % Show Material materials with Cromo of 0.1 % | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Seamless Tube, Tube, Strip, Sheet, Plate, Bar |
Hierro | 0.7 % Show Material materials with Hierro of 0.7 % | H16 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube |
0.70 % Show Material materials with Hierro of 0.70 % | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Magnesio | 0.3 % Show Material materials with Magnesio of 0.3 % | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Seamless Tube, Tube, Strip, Sheet, Plate, Bar |
Manganeso | 0.9 - 1.5 % Show Material materials with Manganeso of 0.9 - 1.5 % | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Seamless Tube, Tube, Strip, Sheet, Plate, Bar |
Silicona | 0.5 % Show Material materials with Silicona of 0.5 % | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Seamless Tube, Tube, Strip, Sheet, Plate, Bar |
Zinc | 0.2 % Show Material materials with Zinc of 0.2 % | H16 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Seamless Tube, Tube, Strip, Sheet, Plate, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good to good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): good, Deep drawing / upsetting (Condition) very good (O) / very good (H12) |