EN 573-3 Grade AW-6005 T4

Want to keep this datasheet? Save it now in your required format

Description

Age-hardenable AlMgSi alloy. The alloy is food safe.

Related Standards

Equivalent Materials

This material data has been provided by WIAM,AluKey.

All metrics apply to room temperature unless otherwise stated. SI units used unless otherwise stated.
Equivalent standards are similar to one or more standards provided by the supplier. Some equivalent standards may be stricter whereas others may be outside the bounds of the original standard.

Ashby charts

See where falls on the material property chart for against in your materials selection and design process. Our Ashby charts are interactive with more technical data upon clicking. Sign up to get access to this premium feature for free.

Properties

General

PropertyValueConditionRelated StandardsShape

Density

2.7 g/cm³

Show Material materials with Density of 2.7 g/cm³

T4

EN 573-3, EN 755

Rod, Tube

Mechanical

PropertyTemperatureValueConditionRelated StandardsShapeComment

Elastic modulus

70.0 GPa

Show Material materials with Elastic modulus of 70.0 GPa

Typical for Wrought 6000 Series Aluminium

Elongation

13.0 %

Show Material materials with Elongation of 13.0 %

T4

EN 573-3, EN 755

Rod, Tube

A50

15.0 %

Show Material materials with Elongation of 15.0 %

T4

EN 573-3, EN 755

Rod, Tube

A100

20.0 °C

13.0 %

Show Material materials with Elongation of 13.0 %

T4

EN 573-3

Profile

A50

20.0 °C

15.0 %

Show Material materials with Elongation of 15.0 %

T4

EN 573-3

Profile

Hardness, Brinell

20.0 °C

50.0 [-]

Show Material materials with Hardness, Brinell of 50.0 [-]

T4

EN 573-3

Profile

Plane-Strain Fracture Toughnes

22.0 - 35.0 MPa·√m

Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m

Typical for Wrought 6000 Series Aluminium

Poisson's ratio

0.33 [-]

Show Material materials with Poisson's ratio of 0.33 [-]

Typical for Wrought 6000 Series Aluminium

Shear modulus

26.0 - 26.5 GPa

Show Material materials with Shear modulus of 26.0 - 26.5 GPa

Typical for Wrought 6000 Series Aluminium

Tensile strength

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

T4

EN 573-3, EN 755

Rod, Tube

20.0 °C

180.0 MPa

Show Material materials with Tensile strength of 180.0 MPa

T4

EN 573-3

Profile

Thermal

PropertyTemperatureValueConditionRelated StandardsShapeComment

Coefficient of thermal expansion

20 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

T4

EN 573-3, EN 755

Rod, Tube

100 °C

2.36e-05 1/K

Show Material materials with Coefficient of thermal expansion of 2.36e-05 1/K

T4

EN 573-3, EN 755

Rod, Tube

Melting point

605.0 - 655.0 °C

Show Material materials with Melting point of 605.0 - 655.0 °C

T4

EN 573-3, EN 755

Rod, Tube

Specific heat capacity

887.0 - 963.0 J/(kg·K)

Show Material materials with Specific heat capacity of 887.0 - 963.0 J/(kg·K)

Typical for Wrought 6000 Series Aluminium

Thermal conductivity

180.0 - 188.0 W/(m·K)

Show Material materials with Thermal conductivity of 180.0 - 188.0 W/(m·K)

T4

EN 573-3, EN 755

Rod, Tube

Electrical

PropertyValueConditionRelated StandardsShape

Electrical conductivity

27000000.0 - 28000000.0 S/m

Show Material materials with Electrical conductivity of 27000000.0 - 28000000.0 S/m

T4

EN 573-3, EN 755

Rod, Tube

Electrical resistivity

3.57e-08 - 3.7e-08 Ω·m

Show Material materials with Electrical resistivity of 3.57e-08 - 3.7e-08 Ω·m

T4

EN 573-3, EN 755

Rod, Tube

Chemical properties

PropertyValueConditionRelated StandardsShape

Chromium

0.1 %

Show Material materials with Chromium of 0.1 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

0.3 %

Show Material materials with Chromium of 0.3 %

T4

EN 573-3

Profile

Copper

0.1 %

Show Material materials with Copper of 0.1 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

0.3 %

Show Material materials with Copper of 0.3 %

T4

EN 573-3

Profile

Iron

0.35 %

Show Material materials with Iron of 0.35 %

T4

EN 573-3

Profile

0.35 %

Show Material materials with Iron of 0.35 %

T4

EN 573-3, EN 755

Rod, Tube

Magnesium

0.4 - 0.6 %

Show Material materials with Magnesium of 0.4 - 0.6 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

0.4 - 0.7 %

Show Material materials with Magnesium of 0.4 - 0.7 %

T4

EN 573-3

Profile

Manganese

0.1 %

Show Material materials with Manganese of 0.1 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

0.5 %

Show Material materials with Manganese of 0.5 %

T4

EN 573-3

Profile

Silicon

0.5 - 0.9 %

Show Material materials with Silicon of 0.5 - 0.9 %

T4

EN 573-3

Profile

0.6 - 0.9 %

Show Material materials with Silicon of 0.6 - 0.9 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

Titanium

0.1 %

Show Material materials with Titanium of 0.1 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

Zinc

0.1 %

Show Material materials with Zinc of 0.1 %

T4

EN 573-3, EN 755

Profile, Rod, Tube

0.2 %

Show Material materials with Zinc of 0.2 %

T4

EN 573-3

Profile

Technological properties

Property
Workability

Excellent workability.