Dimension
Property | Value |
---|---|
Dimensions | Please feel free to check the figure on the right side of the material page for more details. |
Mechanical
Property | Value | Comment |
---|---|---|
Bend allowance | 0 [-] Show Supplier Material materials with Bend allowance of 0 [-] | min. | Transverse | for thickness 0.5-3 mm |
Elongation | 21 % Show Supplier Material materials with Elongation of 21 % | min. | for thickness 0.5-0.7 mm | A80 | Transverse |
22 % Show Supplier Material materials with Elongation of 22 % | min. | for thickness 0.5-0.7 mm | A80 | |
23 % Show Supplier Material materials with Elongation of 23 % | min. | for thickness 0.7-3 mm | A80 | Transverse | |
24 % Show Supplier Material materials with Elongation of 24 % | min. | for thickness 0.7-3 mm | A80 | |
Fatigue strength | 362 MPa Show Supplier Material materials with Fatigue strength of 362 MPa | at 5*10⁶ cycles | for thickness 1 mm |
Tensile strength | 370 - 470 MPa Show Supplier Material materials with Tensile strength of 370 - 470 MPa | for thickness 0.5-3 mm |
380 - 480 MPa Show Supplier Material materials with Tensile strength of 380 - 480 MPa | for thickness 0.5-3 mm | Transverse | |
Yield strength | 280 - 360 MPa Show Supplier Material materials with Yield strength of 280 - 360 MPa | for thickness 0.5-3 mm |
300 - 380 MPa Show Supplier Material materials with Yield strength of 300 - 380 MPa | for thickness 0.5-3 mm | Transverse |
Chemical properties
Property | Value | Comment |
---|---|---|
Aluminium | 0.015 % Show Supplier Material materials with Aluminium of 0.015 % | min. |
Carbon | 0.09 % Show Supplier Material materials with Carbon of 0.09 % | max. |
Manganese | 0.7 % Show Supplier Material materials with Manganese of 0.7 % | max. |
Niobium | 0.09 % Show Supplier Material materials with Niobium of 0.09 % | max. |
Phosphorus | 0.025 % Show Supplier Material materials with Phosphorus of 0.025 % | max. |
Silicon | 0.03 % Show Supplier Material materials with Silicon of 0.03 % | max. |
Sulfur | 0.02 % Show Supplier Material materials with Sulfur of 0.02 % | max. |
Titanium | 0.15 % Show Supplier Material materials with Titanium of 0.15 % | max. |
Technological properties
Property | ||
---|---|---|
Application areas | The steel grade is particularly suitable for structural parts that do not require severe forming (profiling, bending or light drawing): automotive structures and reinforcements, industrial shelving systems, radiators, racking systems, furniture, mechanical engineering applications etc. | |
Coating | Galvanisation: Class 1 | |
Surface condition | Surface cleanliness If improved surface cleanliness is required, ArcelorMittal also offers this steel grade with compulsory use of continuous annealing or hydrogen annealing. | |
Welding | The steel grade has good weldability in all welding processes. Based on many years’ practical experience in arc and resistance spot welding of its products, ArcelorMittal can provide valuable technical assistance in defining the welding parameters for this grade. | |
Workability | Forming limit curves can be used to define the maximum strains not to be exceeded when forming steel by various methods, so as to avoid the risk of incipient necking. These curves are available on request. Please contact for other forming data on this grade for particular sheet thicknesses. |