Dimension
Property | Value |
---|---|
Dimensions | Please feel free to check the figure on the right side of the material page for more details. |
Mechanical
Property | Value | Comment |
---|---|---|
Elongation | 36 % Show Supplier Material materials with Elongation of 36 % | min. | for thickness 0.7-3 mm | Transverse | A80 |
Plastic strain ratio | 1.5 [-] Show Supplier Material materials with Plastic strain ratio of 1.5 [-] | average | for thickness 0.7-3 mm |
Tensile strength | 270 - 350 MPa Show Supplier Material materials with Tensile strength of 270 - 350 MPa | for thickness 0.7-3 mm | Transverse |
Yield strength | 140 - 220 MPa Show Supplier Material materials with Yield strength of 140 - 220 MPa | for thickness 0.7-3 mm | Transverse |
Chemical properties
Property | Value | Comment |
---|---|---|
Carbon | 0.08 % Show Supplier Material materials with Carbon of 0.08 % | max. |
Manganese | 0.5 % Show Supplier Material materials with Manganese of 0.5 % | max. |
Phosphorus | 0.025 % Show Supplier Material materials with Phosphorus of 0.025 % | max. |
Sulfur | 0.05 % Show Supplier Material materials with Sulfur of 0.05 % | max. |
Technological properties
Property | ||
---|---|---|
Application areas | This steel has many applications: | |
Coating | Enamelling Surface preparation: Application of the enamel and firing: Finally, firing is performed at a temperature of about 830°C. | |
Joining | It can be welded without any difficulty, whatever the welding process may be. Other joining processes (clinching, crimping) may also be used. | |
Processing methods | Grade DC05EK EN 10209, which has superior mechanical properties compared with DC04EK EN 10209, is especially intended for forming bathtubs. |